METAL OXIDE OR METAL NITRIDE-COATED STEEL FASTENERS

A fastener assembly and methods for forming a coated fastener are provided. The fastener assembly includes a fastener configured for joining at least two metal parts, and at least one of a metal oxide or a metal nitride dielectric coating disposed on an outside surface of the fastener. The fastener is formed from steel. The at least one of the metal oxide or the metal nitride dielectric coating includes an aluminum-based material and is configured to provide a dielectric barrier between the steel of the fastener and at least one second metal that is different than the steel of the fastener.

Skip to: Description  ·  Claims  · Patent History  ·  Patent History
Description
INTRODUCTION

The present disclosure relates to a coated fastener, and more particularly to a coated steel fastener for joining dissimilar metallic parts.

Magnesium, being a light structural metal, offers high specific strength, stiffness, and excellent shock absorption performance, making it an ideal material for automotive body-in-white (BIW) applications. However, when magnesium is joined with anothermetal such as aluminum or steel, it is prone to galvanic corrosion due to its low (negative) electrochemical potential. In the presence of salt spray or moisture, which acts as an electrolyte, magnesium can easily corrode. This is because magnesium, being more electronegative, will act as an anode and lose electrons to more electropositive metals like aluminum or steel, which act as a cathode. This electrochemical reaction leads to oxidation and subsequent corrosion of magnesium.

In automotive applications, magnesium and aluminum sheets are often joined using bolts and flow drill screws. These bolts are typically made of carbon steel due to its high strength and shear resistance, which are crucial for safety in high-stress applications. However, the introduction of steel bolts creates a galvanic couple with both magnesium and aluminum, exacerbating corrosion issues. To mitigate this, steel bolts are usually coated with zinc-based alloys as zinc is closer to magnesium on the galvanic series and offers better corrosion protection. Alternatively, aluminum bolts can be used, which are less corrosive to magnesium compared to steel bolts.

While present fasteners achieve their intended purpose, there is a need for new and improved fastener that offer improved performance and stability.

SUMMARY

According to several aspects of the present disclosure, a fastener assembly is provided. The fastener assembly includes a fastener configured for joining at least two metal parts, and at least one of a metal oxide or a metal nitride dielectric coating disposed on an outside surface of the fastener. The fastener is formed from steel. The at least one of the metal oxide or the metal nitride dielectric coating includes an aluminum-based material and is configured to provide a dielectric barrier between the steel of the fastener and at least one second metal that is different than the steel of the fastener.

In accordance with another aspect of the disclosure, the fastener is a bolt.

In accordance with another aspect of the disclosure, the steel is carbon steel.

In accordance with another aspect of the disclosure, the at least one second metal includes at least one of magnesium (Mg), iron (Fe), or aluminum (Al).

In accordance with another aspect of the disclosure, a first metal part is magnesium and a second metal part is aluminum.

In accordance with another aspect of the disclosure, the at least one of the metal oxide or the metal nitride dielectric coating includes an inner layer of aluminum (Al) and an outer dielectric layer of Al2O3.

In accordance with another aspect of the disclosure, the at least one of a metal oxide or a metal nitride dielectric coating includes an inner layer of aluminum (Al) and an outer dielectric layer of aluminum nitride (AlN).

According to several aspects of the present disclosure, a method for forming a coated fastener is provided. The method includes applying an aluminum-based metal to a fastener using at least one of electroplating or hot-dip aluminizing, and converting the aluminum-based metal into at least one of a metal oxide or a metal nitride dielectric coating to form the coated fastener with a dielectric coating. The fastener is formed from steel. The dielectric coating is configured to provide a dielectric barrier between the steel of the fastener and at least one second metal that is different than the steel of the fastener.

In accordance with another aspect of the disclosure, the at least one of the metal oxide or the metal nitride dielectric coating includes aluminum oxide (Al2O3).

In accordance with another aspect of the disclosure, the aluminum-based metal includes anodizing the aluminum-based metallic coating.

In accordance with another aspect of the disclosure, the aluminum-based metal includes an anodizing time between 30 minutes and 120 minutes.

In accordance with another aspect of the disclosure, the aluminum-based metal includes anodizing at a voltage between 10 and 40 volts DC.

In accordance with another aspect of the disclosure, the aluminum-based metal includes anodizing with an electrolyte temperature between 5° C. and 20° C.

In accordance with another aspect of the disclosure, the aluminum-based metal includes anodizing with an H2SO4 solution concentration between 10 and 20 weight%.

In accordance with another aspect of the disclosure, the aluminum-based metal includes plasma nitriding the aluminum-based metal.

In accordance with another aspect of the disclosure, plasma nitriding the aluminum-based metal includes argon (Ar+) pre-sputtering the aluminum-based metal to remove a naturally occuring oxide layer at a temperature between 250 °C. and 450° C.

In accordance with another aspect of the disclosure, plasma nitriding the aluminum-based metal is performed at a temperature between 400° C. and 500° C.

In accordance with another aspect of the disclosure, converting the aluminum-based metal includes using a sol gel process to form aluminum oxide (Al2O3) on the fastener.

In accordance with another aspect of the disclosure, the at least one second metal includes a first sheet of magnesium and a second sheet of aluminum.

According to several aspects of the present disclosure, a method for forming a coated fastener is provided. The method includes applying an aluminum-based metal to a fastener using electroplating, and converting the aluminum-based metal into a metal oxide dielectric coating including aluminum oxide (Al2O3) using a hard coat anodizing treatment to form the coated fastener with a dielectric coating. The fastener is formed from steel. The aluminum-based metal includes a first aluminum coating and a second aluminum oxide coating, and the first aluminum coating and the second aluminum oxide coating are between 10 and 30 microns (µm) in total thickness. The dielectric coating is configured to provide a dielectric barrier between the steel of the fastener and at least one of a first sheet of magnesium and or a second sheet of aluminum.

The above features and advantages, and other features and advantages, of the presently disclosed system and method are readily apparent from the detailed description, including the claims, and examples when taken in connection with the accompanying drawings.

BRIEF DESCRIPTION OF THE DRAWINGS

The present disclosure will become more fully understood from the detailed description and the accompanying drawings, wherein:

FIG. 1 is a side cross section view illustrating an example of a fastener assembly, where the fastener assembly includes a fastener with a dielectric coating, in accordance with the present disclosure.

FIG. 2 is a schematic diagram illustrating a method for forming the fastener with the dielectric coating shown in FIG. 1, including electroplating and anodizing or hot-dipping, in accordance with the present disclosure.

FIG. 3 is a schematic diagram illustrating method steps for forming an aluminum oxide layer on the fastener shown in FIG. 1, where the steps include plasma nitriding, in accordance with the present disclosure.

FIG. 4 is a schematic diagram illustrating method steps for forming an aluminum oxide layer on the fastener shown in FIG. 1, where the steps include a sol gel process, in accordance with the present disclosure.

DETAILED DESCRIPTION

The following description is merely exemplary in nature and is not intended to limit the present disclosure, application, or uses. Furthermore, there is no intention to be bound by any expressed or implied theory presented in the preceding introduction, summary, or the following detailed description. It should be understood that throughout the drawings, corresponding reference numerals indicate like or corresponding parts and features.

Reference will now be made in detail to several examples of the disclosure that are illustrated in accompanying drawings. Whenever possible, the same or similar reference numerals are used in the drawings and the description to refer to the same or like parts or steps. The drawings are in simplified form and are not to precise scale. The following description is merely exemplary in nature and is not intended to limit the present disclosure, application, or uses.

A coated fastener and method for forming the fastener is disclosed herein. The use of zinc (Zn)-coated steel bolts and aluminum (Al) bolts in mixed metal joints presents several challenges. First, for galvanic corrosion to occur, there must be an electrical connection between the dissimilar metal parts. Ideally, the coating on the fastener metal should provide a dielectric barrier to block electron transfer from the anode to the cathode. However, metallic coatings like zinc (Zn) still allow electrical connections, increasing the potential for galvanic corrosion. Additionally, Zn is a soft metal, making the Zn coating prone to wear or abrasion, especially in the threaded regions of bolts where high friction and mechanical deformation during installation can cause the coating to delaminate, leaving the threads unprotected against corrosion. On the other hand, Al bolts, being softer than steel, require joint redesigns, such as using larger diameters and modifying bolt spacing, making them more suitable for low-stress applications to prevent bolt damage or failure due to overtightening.

To address these issues, the ideal steel bolt coating should act as a dielectric barrier to prevent electron flow between the Mg (anode) and Fe/Al (cathode). The coating must also possess high strength and abrasion resistance to avoid loss at the head and thread areas during bolt insertion. The fastener disclosed herein proposes a method to develop a hard dielectric coating on steel fasteners (e.g., bolts or flow drill screws) to prevent corrosion in mixed metal joints. The process involves electroplating or applying the bolt with a pure Al layer, followed by partial transformation of the Al layer into aluminum oxide (Al2O3) or aluminum nitride (AlN). This transformation creates a dielectric barrier between the metallic parts, effectively preventing galvanic corrosion.

FIG. 1 illustrates a fastener assembly 10 including a fastener 12 and a metal oxide or metal nitride dielectric coating 14 disposed on an outside surface of the fastener 12. In the view in FIG. 1, the coated fastener 12 is shown coupling a first metal 16 and a second metal 18. The first metal 16 and/or the second metal 18 may be in the form of a sheet.

The fastener 12 may include a carbon steel bolt or screw designed for use in high-stress applications requiring superior strength and durability. The fastener 12 may be characterized by its high tensile strength and shear resistance, making it suitable for securing components in automotive, aerospace, and construction industries. The fastener 12 can feature a threaded shank and a hexagonal head, for example, allowing for easy installation and removal using standard tools. It will be appreciated that the fastener 12 may include and be formed from other suitable metals and materials configured for serving as a fastener.

The dielectric coating 14 is disposed on the outside surface of the fastener 12. To enhance corrosion resistance, the fastener 12 is coated with the dielectric coating 14, which provides a barrier that protects the underlying steel of the fastener 12 from oxidative degradation. Additionally, the dielectric coating 14 ensures uniform coverage, including the threaded regions, to prevent galvanic corrosion when used in conjunction with dissimilar metals, such as aluminum or magnesium. This embodiment offers a reliable and cost-effective solution for joining metal parts while maintaining structural integrity and longevity in demanding environments.

The dielectric coating 14 includes an aluminum-based material, for example aluminum oxide (e.g., Al2O3), configured to provide a dielectric barrier between the steel of the fastener and a magnesium or aluminum sheet in an electrolyte environment (e.g., two metal parts, the first metal 16 and/or the second metal 18). Besides providing a dielectric barrier, the dielectric coating 14 is relatively hard compared to other traditional coatings or materials, such as zinc coatings and aluminum parts (e.g., a bolt). For instance, a zinc coating is particularly prone to wear or abrasion. This can be manifested in form of scratches in the fastener head during handling/installation. Particularly, in a threaded region of a bolt, a zinc coating can delaminate due to high friction and mechanical deformation during the bolt installation. This delamination leaves the threads unprotected against corrosion. When an Al bolt is used, it may be necessary to redesign the joint, such as using a larger diameter and/or modification of bolt spacing. Thus, Al bolts are more suitable to be used in low stress application, where the requirements are low enough to prevent bolt damage or failure due to overtightening.

In an example, the dielectric coating 14 is aluminum oxide (Al2O3). The dielectric coating 14 can be developed by forming an aluminized coating (e.g., aluminum or aluminum alloy) on the fastener 12 followed by an anodizing treatment to the aluminized coating on the surface of the fastener 12 at least partially into an Al2O3 layer. An Al2O3 layer is advantageous because Al2O3 is electrically insulating with a high dielectric strength ranging of 14-16 kilovolts per millimeter (kV/mm). Additionally, the Al2O3 layer has a high hardness (~ 350 Vickers Hardness (HV)) providing wear resistance to the dielectric coating 14.

In another example, the dielectric coating 14 includes multiple layers. For example, the dielectric coating 14 may include a first layer 20 (or inner layer) of aluminum or aluminum alloy and a second layer 22 (or outer layer) of Al2O3. In another example, the dielectric coating 14 may include a first layer 20 (or inner layer) of aluminum or its alloy and a second layer 22 (or outer layer) of aluminum nitride (AlN) (shown in FIG. 2). It will be appreciated that the dielectric coating 14 may include other suitable materials that are dielectric and provide a suitable hardness for fastening dissimilar metals.

As shown in FIG. 1, the electrolyte environment may include the first metal 16 (e.g., a magnesium sheet or other metal part) and a second metal 18 (e.g., an aluminum sheet or other metal part). When magnesium (Mg) is electrochemically coupled with steel (Fe), the magnesium (Mg) acts as an anode and will oxidize and easily lose its electron to the iron side (which functions as a cathode) of the galvanic couple, which causes the magnesium (Mg) to corrode.

FIG. 2 illustrates a method 100 for forming the coated fastener 12 used in the fastener assembly 10 discussed above. The method 100 begins at step 102.

Step 102 depicts applying an aluminum-based metal (aluminum layer 24) to the fastener 12 using at least one of electroplating or hot-dip aluminizing. In this step, the fastener 12 may be cleaned using, for example, abrasive blasting and/or chemical cleaning. In some cases, a zincate treatment may be applied to the fastener 12 to assist in better adhesion with subsequent layers. Additionally, in some instances, an electroless nickel plating may be applied to the fastener 12 to function as a barrier and as a smooth surface for the aluminum plating.

In the case of electroplating, shown in step 102A, the fastener 12 may then be immersed in an electrolyte solution containing aluminum ions. Through an electrolysis process, the aluminum layer 24 is deposited onto the fastener 12. In an example, the aluminum layer 24 may be between 5 to 50 microns in thickness. An anodizing process is used to transform the metallic Al or Al alloydielectric coating layer 14 partially into an aluminum oxide Al2O3 layer. When the dielectric coating 14 includes two layers (e.g., Al and Al2O3), the aluminum layer thickness may be in a range between 5 to 20 microns and the Al2O3 layer thickness is between 10 to 30 microns. After the anodizing treatment, the pores in the anodized layer are sealed by using an organic dye and polymer sealants.

In the case of hot-dip aluminizing, as shown at step 102B, the fastener 12 is immersed in a bath of molten aluminum (Al) or an aluminum-silicon alloy (AlSi) (e.g., aluminum 90 weight percent (wt.%)/silicon 10 wt.%, aluminum 93 wt.%/silicon 7 wt.%) or Al-Mg-Si alloy (containing about 8-10 wt.% Si and 5-15 wt.% Mg). The temperature of the aluminum bath may be around 700° C. (1292° F.). Subsequent to the immersion step, the fastener 12 may be cooled, allowing the resulting aluminum-based metal layer to solidify and form a strong metallurgical bond with the steel of the fastener 12.

Next, step 104 depicts converting the aluminum-based metal into the dielectric coating 14 to form the coated fastener 12. As discussed above, the dielectric coating 14 is configured to provide a dielectric barrier between the steel of the fastener and an electrolyte environment, and the electrolyte environment includes at least one second metal that is different than the steel of the fastener, for example the first metal 16 and/or the second metal 18.

In one example, shown in step 104A, converting the aluminum-based metal into the dielectric coating 14 includes anodizing the aluminum-based metal. Anodization can include an electrolytic passivation process. During anodization of the fastener 12, the fastener 12 having the aluminum metal coating may be submerged and suspended as an anode in an electrolytic solution, for example sulfuric acid, using stainless steel as a cathode. In specific examples, converting the aluminum-based metal using anodizing may include using a voltage between 10 and 40 volts direct current (V DC), an electrolyte temperature between 5 and 20° C., a sulfuric acid (H2SO4) concentration between 10 and 20 wt.%, and/or an anodizing time between 30 and 120 minutes. In an example, the resulting anodized layer of aluminum oxide may be sealed using a sealant and/or nickel acetate, which may or may not include an organic die.

In another example, as illustrated in FIG. 3, converting the aluminum-based metal into the dielectric coating 14 includes a method 300 of plasma nitriding the aluminum-based metal. Plasma nitriding, also known as ion nitriding, includes a thermochemical surface treatment. Often, a naturally forming oxide layer 26 (e.g., Al2O3), shown at step 302, may form on a surface of the aluminum metal layer deposited on the fastener 12. The naturally forming oxide layer 26 may be removed using, for example, argon pre-sputtering of the surface of the aluminum metal layer as shown in step 304. In an example, the argon pre-sputtering may be performed at a temperature between 250 and 450° C. Then, as shown in step 306, plasma nitriding can be performed on the fastener 12 and pre-sputtered aluminum-based metal 24. The plasma nitriding may include exposing the fastener 12 to nitrogen ions (N+) to form a hard aluminum nitride (AlN) layer 28, as shown at step 308. In an example, the plasma nitriding may be performed at a temperature between 400 and 500° C.

As depicted in FIG. 4, converting the aluminum-based metal into the dielectric coating 14 may include a method 400 of using a sol gel process to form aluminum oxide (Al2O3) on the fastener 12. A sol gel process includes a transition of a solution into a gel-like network, which can then be dried and heat-treated to form solid aluminum oxide (Al2O3). Typically, a metal alkoxide, for example aluminum alkoxide, is used as a precursor and dissolved in a solvent to form a solution, as shown at step 402. Next, the fastener 12 is dipped into the solution, which undergoes hydrolysis (step 404) and a polycondensation reaction (step 406) and leads to formation of a colloidal suspension or sol. The sol transitions into a gel of a network of interconnected particles. The fastener 12 is then removed and dried to remove the solvent resulting in a porous solid (step 408). The fastener 12 is then heat-treated to densify and crystallize the porous solid resulting in a coating of aluminum oxide (Al2O3).

The fastener 12 and methods of the present disclosure are advantageous and beneficial over prior art. The fastener 12 disclosed herein proposes a method to develop a hard dielectric coating on steel fasteners (e.g., bolts or flow drill screws) to prevent corrosion in mixed metal joints. The process involves electroplating or applying the bolt with a pure Al layer, followed by partial transformation of the Al layer into aluminum oxide (Al2O3) or aluminum nitride (AlN). This transformation creates a dielectric barrier between the metallic parts, effectively preventing galvanic corrosion while providing a strong coating the prevents delamination at the heads or the threads during fastener installation.

This description is merely illustrative in nature and is in no way intended to limit the disclosure, its application, or uses. The broad teachings of the disclosure can be implemented in a variety of forms. Therefore, while this disclosure includes particular examples, the true scope of the disclosure should not be so limited since other modifications will become apparent upon a study of the drawings, the specification, and the following claims.

Claims

1. A fastener assembly, comprising:

a fastener configured for joining at least two metal parts, wherein the fastener is formed from steel; and
at least one of a metal oxide or a metal nitride dielectric coating disposed on an outside surface of the fastener, wherein the at least one of the metal oxide or the metal nitride dielectric coating includes an aluminum-based material, wherein the at least one of metal oxide or metal nitride dielectric coating is configured to provide a dielectric barrier between the steel of the fastener and at least one second metal that is different than the steel of the fastener.

2. The fastener assembly of claim 1, wherein the fastener is a bolt.

3. The fastener assembly of claim 1, wherein the steel is carbon steel.

4. The fastener assembly of claim 1, wherein the at least one second metal includes at least one of magnesium (Mg), iron (Fe), or aluminum (Al).

5. The fastener assembly of claim 1, wherein a first metal part is magnesium and a second metal part is aluminum.

6. The fastener assembly of claim 1, wherein the at least one of the metal oxide or the metal nitride dielectric coating includes an inner layer of aluminum (Al) and an outer dielectric layer of Al2O3.

7. The fastener assembly of claim 1, wherein the at least one of a metal oxide or a metal nitride dielectric coating includes an inner layer of aluminum (Al) and an outer dielectric layer of aluminum nitride (AlN).

8. A method for forming a coated fastener, comprising:

applying an aluminum-based metal to a fastener using at least one of electroplating or hot-dip aluminizing, wherein the fastener is formed from steel; and
converting the aluminum-based metal into at least one of a metal oxide or a metal nitride dielectric coating to form the coated fastener with a dielectric coating, wherein the dielectric coating is configured to provide a dielectric barrier between the steel of the fastener and at least one second metal that is different than the steel of the fastener.

9. The method of claim 8, wherein the at least one of the metal oxide or the metal nitride dielectric coating includes aluminum oxide (Al2O3).

10. The method of claim 8, wherein converting the aluminum-based metal includes anodizing the aluminum-based metallic coating.

11. The method of claim 10, wherein anodizing the aluminum-based metal includes an anodizing time between 30 minutes and 120 minutes.

12. The method of claim 10, wherein anodizing the aluminum-based metal includes anodizing at a voltage between 10 and 40 volts DC.

13. The method of claim 10, wherein anodizing the aluminum-based metal includes anodizing with an electrolyte temperature between 5° C. and 20° C.

14. The method of claim 10, wherein anodizing the aluminum-based metal includes anodizing with an H2SO4 solution concentration between 10 and 20 weight%.

15. The method of claim 8, wherein converting the aluminum-based metal includes plasma nitriding the aluminum-based metal.

16. The method of claim 15, wherein plasma nitriding the aluminum-based metal includes argon (Ar+) pre-sputtering the aluminum-based metal to remove a naturally occuring oxide layer at a temperature between 250° C. and 450° C.

17. The method of claim 15, wherein plasma nitriding the aluminum-based metal is performed at a temperature between 400° C. and 500° C.

18. The method of claim 8, wherein converting the aluminum-based metal includes using a sol gel process to form aluminum oxide (Al2O3) on the fastener.

19. The method of claim 8, wherein the at least one second metal includes a first sheet of magnesium and a second sheet of aluminum.

20. A method for forming a coated fastener, comprising:

applying an aluminum-based metal to a fastener using electroplating, wherein the fastener is formed from steel; and
converting the aluminum-based metal into a metal oxide dielectric coating including aluminum oxide (Al2O3) using a hard coat anodizing treatment to form the coated fastener with a dielectric coating, wherein the aluminum-based metal includes a first aluminum coating and a second aluminum oxide coating, and wherein the first aluminum coating and the second aluminum oxide coating are between 10 and 30 microns (µm) in total thickness, wherein the dielectric coating is configured to provide a dielectric barrier between the steel of the fastener and at least one of a first sheet of magnesium or a second sheet of aluminum.
Patent History
Publication number: 20260308795
Type: Application
Filed: Apr 7, 2025
Publication Date: Oct 8, 2026
Inventors: Diptak Bhattacharya (Royal Oak, MI), Andrew Clay Bobel (Troy, MI), Ullrich Haus (Brighton, MI), Mary Gilliam (Huntington Woods, MI), Michael J. Lukitsch (Marysville, MI)
Application Number: 19/171,789
Classifications
International Classification: C25D 11/04 (20060101); C23C 8/36 (20060101); C25D 3/44 (20060101); C25D 5/48 (20060101); C25D 7/02 (20060101);