DIRECT POLYMERIZATION, CROSSLINKING AND/OR COVALENT COUPLING OF ENERGETIC MATERIALS

A product, in accordance with one embodiment, includes a polymerized energetic material formed from molecules of at least one energetic material. A product, in accordance with another embodiment, includes a crosslinked energetic material formed from molecules of at least one energetic material. A product, in accordance with another embodiment, includes an energetic material formed from molecules of at least one energetic material covalently coupled together.

Skip to: Description  ·  Claims  · Patent History  ·  Patent History
Description
RELATED APPLICATION

This application claims priority to U.S. Provisional Patent Appl. No. 63/661,772 filed Jun. 19, 2024, which is herein incorporated by reference.

This invention was made with Government support under Contract No. DE-AC52-07NA27344 awarded by the United States Department of Energy. The Government has certain rights in the invention.

FIELD OF THE INVENTION

The present invention relates to energetic materials, and more particularly, this invention relates to polymerization, crosslinking, and/or covalent coupling of energetic materials, and related products.

BACKGROUND

There are many energetic molecules and systems known in the art. Most practical energetic molecules and systems have some degree of both mechanical robustness and stability, allowing relatively safe use. Contrast this with nitroglycerin, which is a liquid that is very sensitive to shock, impact, and spark, rendering its use generally impractical for all but limited purposes. Thus, it is typically desirable for energetic systems to be not only mechanically robust for easier use, but to also have a relatively high stability so that they are not overly sensitive.

Most practical energetics are based predominantly on small molecule, crystalline systems that, on their own, do not have good mechanical properties. To provide both mechanical robustness and stability, many high explosive compositions typically require compounding with a non-energetic polymer ‘binder’ phase or a non-energetic plasticizer to enable pressing or casting into a consolidated, dense, somewhat mechanically robust form with a defined geometry. Consider, for example, TNT, which is relatively stable but has poor mechanical properties. To make TNT in a generally usable form, it is often combined with other things such as organics, polymers, plasticizers, etc. to compound the TNT into a practical form. However, these additives result in reduced performance of the final TNT compound on a volume to volume (vol-vol) basis, in that for every unit of weight of additive included, that unit of weight of TNT is lost per unit volume. Said another way, the TNT is diluted to some extent with the mechanical consolidant.

Non-consolidated neat powders do not approach the maximum hypothetical density of the high energy compound (HE), and therefore, on a vol-vol basis, are not optimal in terms of energetic output.

Furthermore, in many applications where HEs are subject to high stresses, g-loads, and dynamic mechanical environments, powders lack the consolidated strength to maintain shape or location within an assembly. Neat powders may also exhibit reduced safety and stability vs. a pressed consolidated polymer bonded high explosive (PBX).

It is therefore almost always desirable to compound the HE with a binder phase to aid in processing, consolidation, charge formation, and to yield a material with near to hypothetical maximum density and improved mechanical strength and safety. Typically, the binder phase is a polymer with a density that matches the neat HE. However, this severely limits the type of binders which may be employed. Moreover, most binders are non-energetic, e.g., they do not exothermically decompose in the absence of oxygen at elevated temperatures; they are incapable of deflagration nor are they initiable to undergo detonation as with a high explosive, nor do they contribute to overall energetic output of a composite explosive through bond enthalpies, beyond in some scenarios acting as a fuel in later stages of an energetic decomposition. In addition, the binders themselves generally do not crosslink to the HE; rather the binder forms an interpenetrating continuous phase that holds the HE crystals in place mechanically.

In addition, use of binders with densities less than the HE results in reduced performance vol-vol of the final PBX. Binders are parasitic in that for every unit of weight of binder included, that unit of weight of HE is lost. Therefore, the volume of binder is preferably minimized in a given PBX composition.

Plasticizers have similar drawbacks and constraints, with reduced improvements in mechanical properties vs. polymer binders.

A limited number of energetic binders, such as EG nitrocellulose and poly-NIMMO are known in the prior art. However, extant materials are limited in their stability and safety for insensitive HE compositions, such as PBX'd triaminotrinitrobenzene (TATB), and therefore find limited application.

SUMMARY

A product, in accordance with one embodiment, includes a polymerized energetic material formed from molecules of at least one energetic material.

A product, in accordance with another embodiment, includes a crosslinked energetic material formed from molecules of at least one energetic material.

A product, in accordance with another embodiment, includes an energetic material formed from molecules of at least one energetic material covalently coupled together.

BRIEF DESCRIPTION OF THE DRAWINGS

FIG. 1 is a depiction of various molecules of energetic materials, in accordance with various embodiments.

FIG. 2 is a chart illustrating a general reaction space, in accordance with various approaches.

DETAILED DESCRIPTION

The following description is made for the purpose of illustrating the general principles of the present invention and is not meant to limit the inventive concepts claimed herein. Further, features described herein can be used in combination with other described features in each of the various possible combinations and permutations.

Unless otherwise specifically defined herein, all terms are to be given their broadest possible interpretation including meanings implied from the specification as well as meanings understood by those skilled in the art and/or as defined in dictionaries, treatises, etc.

It must also be noted that, as used in the specification and the appended claims, the singular forms “a,” “an” and “the” include plural referents unless otherwise specified.

The following disclosure describes methods of crosslinking, polymerizing and/or otherwise covalently coupling a subset of nitro aromatic, nitramine explosive molecules, and compositions having primary and/or secondary amines via direct reaction of the primary and/or secondary amines with suitable moieties to variously render the system capable of linear polymerization, crosslinking and/or covalent coupling. One advantage of such an approach is that energetic materials (also referred to herein as HEs, energetics, and explosives) may be derived which have significant improvements in mechanical strength and ability to consolidate into a robust form, without the requirement to compound the energetic material with a polymeric binder or a plasticizer species to be monolithic and self-supporting. In various approaches, the modified explosive may be used ‘neat’ (as is) or as a low volume fraction energetic binder phase for another unmodified energetic material. In a further approach, a process may be employed to co-react an energetic material with a polymeric binder to improve mechanical properties and consolidation. Some approaches may be used to create a high explosive surface modifying coupling agent to improve the strength of interaction between HE particles themselves and/or with an existing binder.

In one general embodiment, a product includes a polymerized energetic material formed from molecules of at least one energetic material.

In another general embodiment, a product includes a crosslinked energetic material formed from molecules of at least one energetic material.

In another general embodiment, a product includes an energetic material formed from molecules of at least one energetic material covalently coupled together.

More detailed information is provided below.

Many explosives currently in use contain both amine and nitro functionality in a common core molecule. The explosive material itself may be a small molecule, crystalline system. The inventors have discovered that, contrary to popular wisdom in the art, a subset of these explosives that contain secondary and/or primary amines (e.g., TATB, 2,6-Diamino-3,5-dinitropyrazine-1-oxide (LLM-105) 1,1-diamino-2,2-dinitroethene (FOX7), and nitroguanidine) present a potentially beneficial opportunity to perform reactions with the reactive primary and/or secondary amine. Representations of some of these molecules are shown in FIG. 1.

While the reactivity of primary and secondary amines on such systems has been documented via Mannich type reactions, the suggestion or use of coupling reactions of the amines on an energetic material for the purposes of polymerization, crosslinking, or coupling of an energetic system derived from these processes has not been considered, nor shown to be viable or advantageous previously. In fact, prior to the present disclosure, the accepted wisdom in the art was that the amines on energetic materials were essentially unusable, and moreover, that any reaction affecting the amine of an energetic material would dislodge and/or disrupt the nitro groups, thereby nullify the energetic nature of the material entirely. Accordingly, the inventors have proceeded contrary to the understandings, expectations and accepted wisdom in the art in developing the many aspects provided in the present disclosure. Moreover, the aforementioned understandings, expectations, and common wisdom in the art demonstrate the unpredictability of the various aspects of the present invention presented herein.

Self-crosslinking, crosslinking, and/or linear or branch polymerization directly of energetic materials enables formulation of a new class of binder-free high explosive compositions, energetic binder-bound high explosive compositions, and others, which present many advantages in overall performance and mechanical properties vs. the state of the art PBX compositions. In some approaches, the explosive compositions linearly polymerized are high molar mass systems, and in other approaches, thermoset compositions may be of effectively infinite molar mass (to the extent of HE material present).

Of particular import is that the energetic qualities of the original energetic material are preserved, while the end product is a polymerized, crosslinked, or otherwise self-supporting mass, providing many advantages such as having enhanced mechanical properties relative to a small molecule, crystalline solid. Further advantages include being self-supporting when formed into a monolith, which is not possible with raw powdered forms of the HE in the absence of a binder.

One general aspect of the present invention includes processes for synthesizing polymeric (cross-linked thermoset, linear, and/or branched polymer) energetic compounds from energetic materials having primary and/or secondary amine functionalization, including but not limited to TATB, DAPO, FOX7, or nitroguanidine energetics. Note that nitroguanidine has both primary and secondary amines. A broad general advantage of such an approach is that a dense, consolidated, formable and mechanically robust HE part may be manufactured without the need to dilute the HE with a polymeric binder phase or plasticizer, thereby yielding new HEs with altered performance and/or new compositions based on current HE materials with enhanced output and/or modified response.

Amine functional energetic molecules are generally reactive toward aldehyde-based (e.g., formaldehyde) and isocyanate-based (e.g., toluene diisocyanate (TDI)) coupling reactions, where the aldehyde or isocyanate group(s) form a —N—R—OH termination or a urea coupling directly.

In other approaches, reactions of amines via other types of chemistries (e.g., reactions with oxiranes or alcohols) may be utilized to couple with the amine groups on the energetic compound.

In further approaches, a cyanate ester may be utilized as the reactant to effect coupling with the amine groups on the energetic compound. Cyanate esters tend to be directly reactive with the amines. In some approaches, a catalyst, of a known type such as a transition metal salt or complex e.g. CU(II)ACAC or Ni(II) carboxylates that would become apparent to one skilled in the art after reading the present disclosure, may be added in an effective amount to enhance the cyanate cyclization process.

In general, the amount of the reactant (e.g., aldehyde, isocyanate, alcohol, etc.) that is applied to the HE materials is an effective amount of reactant to achieve a particular end product, as would be determinable by one skilled in the art after reading the present disclosure. Moreover, in some approaches, by controlling the reaction kinetics, one can favor linear systems or favor thermosets. This provides an advantage in that the ability to favor one type of linking over another for a given starting material enables tunability of the properties of the end product.

In some approaches, if a direct 1:1 coupling approach is used, as in the case with an isocyanate, then a stoichiometrically balanced reaction of species with n of 2 or above of isocyanate functionality is required on the isocyanate molecule and an n of 2 or above of primary or secondary amine functionality on the parent molecule are required to form a polymeric system (linear in the case of n=2 for both reactants, cross-linked if n=3 or more for either component and branched if a stoichiometric imbalance and/or a third monofunctional terminator species is introduced into the system). Moreover, it has been observed experimentally that, for isocyanate reactions, the longer and hotter the reaction is allowed to progress, the more likely a primarily linear polymer dominates the product.

If an aldehyde coupling approach is utilized, then each amine is capable of being transformed into 1-2 N—R—OH terminations depending on the primary, secondary character and the control of the aldehyde reaction conditions (stoichiometric control). In any case, the first product of the reaction with the aldehyde is non-polymeric. This first product is capable of polycondensation into a linear, branched and/or crosslinked thermoset system on the addition of heat under appropriate catalytic conditions. This process is potentially advantageous for current PBX processes because it allows the formation of a room temperature stable, soluble energetic ‘molding powder’ which may be lacquered and/or prilled with unmodified HE, or pressed ‘neat’ (preferably with heating) whereupon it crosslinks during pressing to form a mechanically robust thermoset composite or neat thermoset. The neat thermoset would thus comprise the HE, as reacted, in some approaches.

Thermosets provide good mechanical properties, especially when used under long term loads where effects such as creep are an issue. Creep can be substantially eliminated in thermosets under load due to the crosslinking.

Note that in some approaches, it may be preferable to consolidate the powder prior to inducing crosslinking, e.g., by pressing, and then inducing crosslinking of the consolidated powder, e.g., while in the press.

Branched or linear direct couple or condensable systems may be used in a similar way to current non-energetic polymer binders in prilling processes with the advantages of density matching and energetic output, but without the advantages of crosslinking, unless a latent, crosslinkable moiety is included in the structure. Such branched or linear direct couple or condensable systems may be akin to thermoplastics, where they may be formed into various shapes upon heating. Moreover, such branched or linear direct couple or condensable systems may also function well as energetic binders.

Energetic materials may be combined to form a hybrid material. Accordingly, a polymerized energetic material may be formed from molecules of at least two different energetic materials polymerized together. Likewise, a crosslinked energetic material may be formed from molecules of at least two different energetic materials crosslinked together. In further embodiments, an energetic material is formed from molecules of at least two different energetic materials covalently coupled together.

In some approaches, a composite is formed by intermixing a first HE (e.g., as a prilling powder or other crosslinked, polymerized, or covalently coupled HE) along with one or more additional components, such as unmodified first HE, another HE (modified or unmodified), etc. in a composite and/or reacted/coupled together. The first HE may or may not be reacted with the other component(s). In some approaches, the first HE may be present at about 1 wt % to about 20 wt % of the composite (especially when used as a binder for the unmodified first HE or another HE). In other approaches, more of the first HE may be present, e.g., up to about 50 wt %, up to about 75 wt %, up to about 99 wt % based on a total weight of the composite. For example, the first HE may be used as an energetic binder to PBX the bulk HE in the composite, e.g., a nitroguanidine polymer used as a binder for PTAB, a DAPO based polymer used as a binder for DAPO, etc. Because the binder based on the first HE is energetic, more binder may be used than would have been used in a conventional PBX while not losing significant energy per unit volume, thereby enhancing the mechanical robustness of the composite.

Rapidly reactive direct couple systems to form thermosets (e.g., N=3 isocyanates) may be of use as binders or neat materials for reactive, castable HE compositions. As mentioned above, extant HE systems use non-energetic binders such as urethanes or epoxies to bind RDX and/or high melting explosive (HMX) and other materials.

The same direct couple approach(es) may also be utilized to add a percentage (e.g., about 5 to about 99 wt %) of mono-or di-terminated long chain elements to the energetic molecule core as a neat system or an additive to a highly crosslinked, high glass transition temperature (Tg) system to moderate the Tg and provide some elastomeric character to an otherwise rigid energetic system, which may otherwise suffer from increased friction and impact sensitivity, deflagration, and/or unwanted detonation. A high Tg is considered greater than 100 °C, while a moderate Tg is between room temperature and 100 °C. HE materials with a high Tg tend to exhibit more sensitivity to impact and/or friction than at lower Tgs, e.g., in terms of stability, safety, etc. Therefore, such materials can be made safer by reducing the Tg as presented herein.

As alluded to above, in some approaches, kinetic control may be used to favor polymerization or thermoset. For example, many of the reactions described herein are performed at 80 °C or higher. In some cases, temperatures in lower ranges above 80 °C (e.g., 80 °C to 100 °C) may favor formation of thermoset species, while relatively higher temperatures may favor linear polymer species.

The reactions may be performed in solution. For reactions based on an aldehyde, the reaction may be performed in the aldehyde. For reactions based on epoxide, the energetic material may be dissolved in a suitable solvent such as dimethyl sulfoxide (DMSO) at elevated (above room temperature), then the resin (epoxide) is added and the mixture is refluxed or heated for a period of time, and is then processed to crash the product out of solution to obtain the product. For a pre-polymer product (if going for thermoset), the product can be extracted prior to significant linking. For a polymerized product (e.g., linear product), the reaction can be allowed to go to completion.

While most of the HE materials listed herein will react with the reactant slowly without catalyst, an effective amount of a catalyst that improves the speed of reaction may be used. Examples of such catalysts include organo-tin salts (e.g. tin(II)ethylhexanoate for isocyanate coupling processes; transition metal complexes for cyanate ester couplings (e.g. Ni(II)carboxylates); Lewis acids, bases or amines for epoxy-based coupling (e.g. boron trifluoride monoethylamine or triethylenetetramine); etc.

In approaches where a liquid resin is present, the reaction may be performed by mixing the neat HE material into the resin with, but preferably without, adding solvent to maximize density and minimize process complexity.

The general approaches to coupling described herein may also be used to surface-functionalize otherwise unmodified HE particles to increase wettability, interaction strength between particles (ultimate strength of the composite), and/or render the HE reactive toward a polymeric binder for the purposes of coupling. Thus, for example, rather than bulk polymerization of the HE material, the amines located along the surfaces of the HE particles may be caused to crosslink with amines located along the surfaces of other HE particles.

In another example, the amines located along the surfaces of the HE particles may be caused to crosslink and/or couple with a binder resin (whether the resin is energetic or not). Thus, in this example, rather than mechanical coupling of the HE particles with the binder, a chemical bond directly between the HE particles and the binder is created.

In some approaches, thermoset aldehyde reacted systems may also be co-condensed with species such as cyanurates, polyamines (e.g., melamine), epoxies, or unmodified energetic materials to form a networked system with potential advantage, such as tailored mechanical and physical properties. In addition, such composites may be created to dilute the energetic contribution of the material and/or to reduce the sensitivity to initiation. Thus, if a material is extremely energetic and too sensitive in its neat form to be used safely, it may be co-polymerized with another system to create an interpenetrating network, co-network, etc. to stabilize the system while retaining some degree of energetic output. Cyanurate may be used to create systems having very high thermal stability, good mechanical properties, good resistance to water uptake, and other beneficial properties. This was confirmed experimentally. Polyamines impart good thermal stability and mechanical properties. Epoxies tend to provide moderate thermal stability and mechanical property improvements, but in general provide no energetic synergy, and thus are useful as an energetic diluent. As in all composite systems recited herein, the relative amounts of the constituents may be selected to provide a desired set of properties.

In further approaches, a HE starting material may be co-polymerized with up to about 75 wt % of a nitrogen-rich material that is not energetic on its own (i.e., prior to co-polymerization), relative to the weight of the copolymer, to acquire energetic participation by the non-energetic material as part of the co-polymer network. The inventors surprisingly found that in such approaches, the co-polymerized nitrogen-rich material of the networked system provides energetic participation in the decomposition, enhancing the energy output far above what was expected. This result was not predictable.

In some embodiments, a nitrogen-rich material may be one having a ratio of nitrogen atoms to other atoms of at least 1:10, preferably at least 1:5.

To elaborate, consider a system having 25 wt % of a HE material combined with a non-energetic nitrogen-rich material that forms the remaining 75 wt % of the system. One would expect the system to provide an energy output corresponding to only the 25 wt % of the HE material. However, as was surprisingly discovered, when the two materials are polymerized with or crosslinked into respective interpenetrating networks, the non-energetic component exhibits energetic participation in the exothermic thermal decomposition of the system.

In some approaches, the crosslinked energetic material is formed from molecules of the at least one energetic material and a non-energetic binder crosslinked together. For example, a catalyst may be used to favor cross reactions of the co-networks. For example, if making a cyanurate-based system, the energetic material may be present in a lower (or higher) stoichiometric ratio, which reacts quite quickly. The resulting network may be crosslinked to the non-energetic co-network via a nickel-based catalyst that induces the crosslinking, e.g., via cyclotrimerization.

In other approaches based on epoxides, epoxides tend to react with the amines at room temperature. Therefore, in an analogous method to that in the previous paragraph, and there are excess epoxies present, and one wants to complete the network, and all of the amines have been consumed, then a ring opening polymerization catalyst may be used. Illustrative ring opening polymerization catalysts include, but are not limited to boron salts, rare earth triflates, Lewis acid systems, etc.

Experimental and Illustrative Methodology for Fabrication of Polymerized HEs, Crosslinked HEs, and Covalently Bonded HEs

FIG. 2 illustrates a general reaction space, in accordance with various approaches. As an option, the approaches shown may be implemented in conjunction with other approaches, such as those shown in the other FIGS. described herein and/or in U.S. Provisional Patent Appl. No. 63/661,772, which has been incorporated by reference. Of course, however, these approaches and others presented herein may be used to create materials which may or may not be related to the illustrative embodiments listed herein. Further, the methodology implied in FIG. 2 and elsewhere herein may be carried out in any desired environment. Moreover, more or less operations than those shown in FIG. 2 may be included in various approaches. It should also be noted that any of the aforementioned features may be used in any of the embodiments described in accordance with the various methods.

The chart of FIG. 2 illustrates exemplary starting material(s), polymerization type, linking chemistry, binder phase(s), HE phase(s), and the desired property. Many different structures and systems are possible, depending on the selection(s) from some or all of the columns of the chart in FIG. 2 selected for a given approach. In each possible scenario, at least an effective amount of the selected component(s) is used in the particular process. FIG. 10 of U.S. Provisional Patent Appl. No. 63/661,772 and related description therein, which has been incorporated by reference, illustrates an exemplary scenario using the chart of present FIG. 2.

With reference to U.S. Provisional Patent Appl. No. 63/661,772, which has been incorporated by reference, FIGS. 2-8 of U.S. Provisional Patent Appl. No. 63/661,772 and related description therein describe an experiment conducted for a condensable thermoset system.

FIG. 9 of U.S. Provisional Patent Appl. No. 63/661,772 and related description therein describes a general reaction space, in accordance with various approaches.

FIG. 10 of U.S. Provisional Patent Appl. No. 63/661,772 and related description therein describes an example in which a LLM-105 nitroaromatic amine is polymerized into a thermoset phase using oxiraine-amine coupling forming a reactive, crosslinkable co-polymer which may be compounded with a neat HE phase of TATB to form a final crosslinked composite.

An illustrative explanation of reaction stoichiometry and the thermoset-linear product spectrum is described in U.S. Provisional Patent Appl. No. 63/661,772, which has been incorporated by reference, with relation to FIG. 11 of U.S. Provisional Patent Appl. No. 63/661,772.

FIG. 12 of U.S. Provisional Patent Appl. No. 63/661,772 and related description therein describes the stepwise addition of NH-groups with cyanates and isoureas.

FIG. 13 of U.S. Provisional Patent Appl. No. 63/661,772 and related description therein describes a summary of the thermal reaction space with cyanate ester species.

In summary of the guidance of FIGS. 9-13 of U.S. Provisional Patent Appl. No. 63/661,772 and related description therein, and the exemplary synthetic schemes presented in U.S. Provisional Patent Appl. No. 63/661,772, the following findings are presented:

    • Cyanate Esters (CEs) and aromatic amines are reactive; this includes the nitro-substituted aromatics of interest
    • Even in the absence of complicating factors, aromatic amines and CEs are capable of a range of reactions that can generally be driven toward cyclo-trimerization of mixed products, but can also clearly form what are believed to be polyimide chains
    • Various substitution and elimination reactions are in play that may lead to greater or lesser ratios of amine aromatic to CE in a given isolated product, regardless of starting reaction ratio
    • Direction of products may be controlled by close control of reaction conditions

In Use:

Various aspects of the present invention may be performed and/or used for any suitable purpose taught or suggested herein.

For example, various aspects described herein enable mechanical stabilization and improvement of high-explosive compositions, as well as formation of energetic binders. Further approaches provide high explosive compositions with improved overall output due to the elimination of passive polymeric binder or plasticizer phases.

In further approaches, the improvements described herein may be applied to munitions applications for improved performance.

In yet other approaches, various aspects may be used to advantage in the mining and/or hydraulic industries.

In further approaches, the aforementioned energetic/reactive ‘molding powder’ may be utilized in lacquering/prilling operations, solution or film cast, spun cast or otherwise. If desired, the reactive molding powder product may be taken to elevated temperature and pressure to condense into a high polymer (high molar mass polymer) or a high polymer thermoset system.

The inventive concepts disclosed herein have been presented by way of example to illustrate the myriad features thereof in a plurality of illustrative scenarios, embodiments, and/or implementations. It should be appreciated that the concepts generally disclosed are to be considered as modular, and may be implemented in any combination, permutation, or synthesis thereof. In addition, any modification, alteration, or equivalent of the presently disclosed features, functions, and concepts that would be appreciated by a person having ordinary skill in the art upon reading the instant descriptions should also be considered within the scope of this disclosure.

While various embodiments have been described above, it should be understood that they have been presented by way of example only, and not limitation. Thus, the breadth and scope of an embodiment of the present invention should not be limited by any of the above-described exemplary embodiments, but should be defined only in accordance with the following claims and their equivalents.

Claims

1. A product comprising a polymerized energetic material formed from molecules of at least one energetic material.

2. The product of claim 1, wherein the polymerized energetic material is primarily a linear polymer.

3. The product of claim 1, wherein the polymerized energetic material is primarily a branched polymer.

4. The product of claim 1, wherein the polymerized energetic material is formed from molecules of at least two different energetic materials polymerized together.

5. The product of claim 1, wherein the polymerized energetic material is formed from molecules of the at least one energetic material and a non-energetic binder polymerized together.

6. The product of claim 1, consisting essentially of the polymerized energetic material, wherein the product is monolithic and self-supporting, wherein no binder is present in the product.

7. The product of claim 1, comprising a second energetic material intermixed with the polymerized energetic material thereby forming a composite, wherein the polymerized energetic material is present at about 1 wt % to about 99 wt % of the composite.

8. The product of claim 7, wherein the polymerized energetic material is present in a range of about 1 wt % to about 20 wt % of the composite.

9. The product of claim 1, comprising a nitrogen-rich material co-polymerized with the at least one energetic material, wherein the nitrogen-rich material is not energetic prior to co-polymerization, wherein the co-polymerized nitrogen-rich material exhibits energetic participation during energetic decomposition of the product.

10. A product comprising a crosslinked energetic material formed from molecules of at least one energetic material.

11. The product of claim 10, wherein the crosslinked energetic material is formed from molecules of at least two different energetic materials crosslinked together.

12. The product of claim 10, wherein the crosslinked energetic material is a composite formed from molecules of an unmodified energetic material and up to about 50 wt % of the molecules of the at least one energetic material based on a total weight of the composite.

13. The product of claim 10, consisting essentially of the crosslinked energetic material, wherein the product is monolithic and self-supporting, wherein no binder is present in the product.

14. The product of claim 10, wherein the crosslinked energetic material is formed from molecules of the at least one energetic material and a non-energetic binder crosslinked together.

15. The product of claim 10, comprising a second material selected from the group consisting of a cyanurate, a polyamine, an epoxy, and an unmodified energetic material combined with the crosslinked energetic material in a networked system.

16. The product of claim 10, comprising a second energetic material intermixed with the crosslinked energetic material thereby forming a composite, wherein the crosslinked energetic material is present at about 1 wt % to about 99 wt % of the composite.

17. A product comprising an energetic material formed from molecules of at least one energetic material covalently coupled together.

18. The product of claim 17, wherein the energetic material is formed from molecules of at least two different energetic materials covalently coupled together.

Patent History
Publication number: 20260337123
Type: Application
Filed: Jun 17, 2025
Publication Date: Oct 29, 2026
Inventors: James Lewicki (oakland, CA), George E. OVERTURF (Brentwood, CA)
Application Number: 19/241,265
Classifications
International Classification: C06B 25/00 (20060101);