METHOD FOR TREATING A COMPOSITION COMPRISING AN OIL DERIVED FROM PLASTIC WASTE

- TotalEnergies OneTech

The present invention relates to a method for treating a composition comprising a liquefied-plastic oil, said composition containing at least 5 ppm by mass of silicon and/or at least 2 ppm by mass of chlorine, as measured according to the ISO20884 standard, said method comprising: a) a step of bringing said composition into contact, under hot conditions, with a strong base; c) a step of washing with a polar solvent that is immiscible with the product obtained, said polar solvent being chosen from water, a polar organic solvent, and mixtures thereof; d) a step of mixing the product of the preceding step with a petroleum product comprising at least one petroleum distillation fraction, the mixture obtained comprising between 1% by mass and 98% by mass of the product of the preceding step; then e) a step of catalytic hydrotreatment in the presence of hydrogen of the mixture obtained in the preceding step.

Skip to: Description  ·  Claims  · Patent History  ·  Patent History
Description
CROSS REFERENCE TO RELATED APPLICATIONS

The present application is a U.S. National Phase application under 35 U.S.C. § 371 of International Patent Application No. PCT/EP2023/079828 filed Oct. 25, 2023, which claims priority of French Patent Application No. 2211075 filed Oct. 25, 2022. The entire contents of which are hereby incorporated by reference.

FIELD

The present invention relates to a method for treating a composition comprising a liquefied-plastic oil, produced in particular from plastic waste.

The chemical recycling of plastic waste, for example via pyrolysis, allows the recovery of this type of waste. The material is thermally decomposed to obtain a hydrocarbon oil containing different impurities, in particular compounds comprising metals and/or heteroatoms such as silicon, chlorine, nitrogen and oxygen.

It is advantageous to treat oils derived from plastic waste so that they can be used as fuel e.g. for combustion engines.

BACKGROUND

For this purpose, hydrotreatments or hydrorefining refer to catalytic treatment processes in the presence of hydrogen, preferably under heat and/or pressure. Hydrotreatment allows the removal of numerous impurities such as unsaturated hydrocarbons, metals and compounds comprising heteroatoms. Hydrotreatments particularly come under known refining processes of petroleum fractions for the production of fuels, as described for example in document WO2014/096704.

However, some impurities contained in oils derived from plastic waste cause deactivation of the catalysts used for hydrotreatment and/or cause operational problems such as fouling and corrosion. These impurities inter alia include chlorine and silicon, in particular in the form of siloxanes.

To refine oils derived from plastic waste with a conventional hydrotreatment method, it is possible previously to mix these oils with a petroleum product of the type petroleum distillation fraction. This type of process is known as co-processing.

To limit deactivation of hydrotreatment catalysts and operational problems in existing processes/units, the quantity of oil mixed with a petroleum product generally does not exceed 1 to 2% by mass. Said restriction strongly limits the prospects of recycling oils derived from plastic waste.

Applications FR 21 04616, FR 21 04617 and FR 21 09395, not yet published by the Applicant, describe a method for purifying plastic pyrolysis oils prior to a steam cracking step. This purification method allows a drastic decrease in the content of compounds comprising heteroatoms and silicon.

SUMMARY

It is the objective of the present invention to feed the oils thus purified into hydrotreatment processes in a mixture with petroleum products.

DETAILED DESCRIPTION

For this purpose, the subject of the invention is a treatment method of the aforementioned type wherein: the composition comprising a liquefied-plastic oil contains at least 5 ppm by mass of silicon as measured according to standard ISO20884 and/or at least 2 ppm by mass of chlorine as measured according to standard ASTM D7359; and the method comprising the following steps

    • a) a contacting step, under heat, of the composition with a strong base;
    • c) a washing step with a polar solvent immiscible with the product obtained, said polar solvent being chosen from among water, an organic polar solvent and mixtures thereof;
    • d) a mixing step of the product from the preceding step with a petroleum product comprising at least one petroleum distillation fraction, the mixture obtained comprising between 1% by mass and 98% by mass of the product from the preceding step; then
    • e) a catalytic hydrotreatment step, in the presence of hydrogen, of the mixture obtained at the preceding step.

In the present description, the term «liquefied-plastic oil» refers to liquid products obtained after treating thermoplastic, thermosetting or elastomer polymers, alone or in a mixture, and generally in the form of waste. The treatment is pyrolysis for example or HydroThermal Liquefaction (HTL). The treated plastic for example is polyethylene, polypropylene, polystyrene, a polyester, polyamide, polycarbonate or mixtures thereof.

Pyrolysis is a thermal cracking process which may or may not be implemented in the presence of a catalyst.

The composition of the liquefied-plastic oil is dependent on the type of treated plastic and is typically formed of more than 80% by mass of hydrocarbons having 1 to 150 carbon atoms. Liquefied-plastic oils particularly contain compounds of paraffin, iso-paraffin, diene, alkyne, olefin, naphthene and aromatic type.

Liquefied-plastic oils also contain impurities such as chlorinated, oxygenated and/or silylated organic compounds, metals, salts, phosphorus-, sulfur- and nitrogen-containing compounds.

In one advantageous embodiment, the composition comprising a liquefied-plastic oil comprises at least 25% by mass of liquefied-plastic oil, preferably at least 50% by mass of liquefied-plastic oil, more preferably at least 90% by mass of liquefied-plastic oil. In one particular embodiment, the composition solely comprises a liquefied-plastic oil.

In one advantageous embodiment, the composition comprising a liquefied-plastic oil additionally comprises an oil derived from biomass. Said oil derived from biomass is chosen for example from among: Panicum virgatum oil, a tall oil (derived from the paper industry), a used cooking oil, an animal fat, a vegetable oil such as rapeseed oil, canola oil, castor oil, palm oil, soybean oil, an algae-extracted oil, an oil extracted from fermentation of oleaginous microorganisms such as oleaginous yeasts, a biomass pyrolysis oil such as lignocellulosic biomass e.g. oil from the pyrolysis of wood, paper and/or cardboard, an oil obtained by pyrolysis of ground waste furniture boards, a pyrolysis oil of elastomers e.g. optionally vulcanised latex, or tyres, and mixtures thereof.

In the present description, it is considered that the composition subjected to the method of the invention initially contains at least 5 ppm by mass of silicon as measured according to standard ISO20884, and/or at least 2 ppm by mass of chlorine as measured according to standard ASTM D7359. Silicon is particularly contained in liquefied-plastic oils in the form of siloxanes, in particular cyclic siloxanes of type D3, D4 and/or D5. Chlorine is particularly contained in liquefied-plastic oils in the form of inorganic chlorine, but also organic chlorine such as chloroethane, dichloroethane, chlorobenzene or vinyl chloride.

In one advantageous embodiment, the strong base at the contacting step a) comprises an oxide, a hydroxide, bicarbonate or alcoholate of an alkali metal cation or alkaline-earth metal cation, or a hydroxide or bicarbonate of a quaternary ammonium cation, alone or in a mixture. More preferably, the strong base is chosen from among LiOH, NaOH, CsOH, Ba(OH)2, Na2O, KOH, K2O, CaO, Ca(OH)2, MgO, Mg(OH)2, NH4OH, TMAOH, TEAOH, TBuOH, MeONa, EtONa and mixtures thereof. Further preferably, the strong base is chosen from among KOH, NaOH and mixtures thereof.

As a variant, the strong base is chosen from among Na2O, K2O, CaO, MgO and mixtures thereof with each other and/or with the previously cited hydroxide bases.

An example of estimating a minimum quantity of strong base to be used at step a) is described below.

In one advantageous embodiment, the contacting step a) is performed at a temperature of at least 85 °C, more preferably at least 100 °C, further preferably at least 150 °C, still further preferably at least 180 °C.

Preferably, the contacting step a) is conducted at a pressure of between 1 bar and 50 bar, more preferably between 1 bar and 30 bar, further preferably of between 1 bar and 25 bar.

The contacting time of step a) is preferably at least 1 mn, more preferably between 5 mn and 2 h, further preferably between 10 mn and 1 h.

In a first advantageous embodiment, the contacting step a) is performed in the presence of water. Preferably, step a) is performed in the presence of a concentrated aqueous solution of the strong base, more preferably in the presence of a saturated aqueous solution of the strong base.

In a second advantageous embodiment, the contacting step a) is performed in the presence of an organic polar solvent comprising an alcohol function and/or ether function. Preferably, said organic polar solvent is chosen from among (i) C1 to C4 alcohols, preferably from among methanol, ethanol, propan-1-ol, propan-2-ol, butan-1-ol, butan-2-ol, 2-methylpropan-1-ol ethylene glycol, propylene glycol, (ii) alcohols having an ether function, preferably diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol and (iii) cyclic ethers, preferably tetrahydrofuran, 2-methyltetrahydrofuran, cyclopentyl methylether, tetrahydropyran, 1,4-dioxane, eucalyptol; and mixtures thereof.

The term “organic polar solvent” in the meaning of the present description covers all chemical species, alone or in a mixture, able to solvate a composition comprising a liquefied-plastic oil, and comprising at least one carbon-hydrogen, carbon-halogen, carbon-chalcogen or carbon-nitrogen covalent bond, and having a nonzero dipolar moment.

In a third advantageous embodiment, the strong base at the contacting step a) is in solid form, e.g. in the form of sodium hydroxide pellets.

In one embodiment, the treatment method, between steps a) and c), comprises a step b) to separate the composition from the strong base.

Said separation step b) is implemented with any method known to skilled persons, inter alia centrifugation, decantation, filtration or a combination of these methods.

Preferably, if the treatment method is conducted in a reactor, the strong base recovered at step b) is recycled back to the head of said reactor for step a).

In the first and second advantageous embodiments described above for step a), the separation step b) allows the separating of a first liquid so-called oily phase corresponding to the product obtained after step a), and a second liquid phase containing most of the strong base. In the third advantageous embodiment described above for step a), the separation step b) allows the separating of a liquid phase corresponding to the product obtained after step a), and a solid phase comprising most of the strong base.

In one variant of embodiment, the mixture formed by the composition and the strong base at step a) is directly subjected to the washing step c). The omission of step b) is advantageous for example in the event that a quantity of strong base is chosen to be in slight excess relative to the minimum quantity for which the calculation method is described below.

In the present description, in particular concerning the washing step c), it is considered that a polar solvent is immiscible with the product resulting from step b) if the recovery rate thereof is higher than or equal to 0.95. The recovery rate is defined as the ratio of volume of extract to the volume of initial solvent, this extract being a phase containing the solvent immiscible with the composition containing a liquefied-plastic oil, and recovered after mixing and decanting a mixture of one part per volume of solvent with twenty-five parts per volume of composition containing a liquefied-plastic oil to be purified, at atmospheric pressure and at a temperature of 20 °C. A method for determining the recovery rate is described for example in application FR2109395 cited previously.

In one embodiment in which the polar solvent at the washing step c) comprises an organic polar solvent, said organic polar solvent is advantageously chosen from among (i) glycol ethers particularly including polyethylene glycol of chemical formula HO—(CH2—CH2—O)n—H with weight average molecular weight of 90 to 800 g/mol, e.g. diethylene glycol and tetraethylene glycol, polypropylene glycol of chemical formula H[OCH(CH3)CH2]nOH with weight average molecular weight of 130 to 800 g/mol, e.g. dipropylene glycol and tetrapropylene glycol, (ii) dialkyl formamides in which the alkyl group may comprise from 1 to 8 or 1 to 3 carbon atoms, in particular N,N-dimethyl formamide (DMF), (iii) dialkyl sulfoxides in which the alkyl group may comprise from 1 to 8 or 1 to 3 carbon atoms in particular dimethylsulfoxide (DMSO) and sulfolane, (iv) compounds comprising a furan ring, (v) cyclic carbonates esters particularly having 3 to 8 or 3 to 4 carbon atoms, in particular propylene carbonate and ethylene carbonate; and mixtures thereof.

In one advantageous embodiment, the polar solvent at the washing step c) is water at neutral pH (pH=7) or acid pH (pH<7). Preferably, said water does not contain a base and in particular a hydroxide base. The acid pH of the water is obtained for example by adding one or more organic or inorganic acids. Examples of organic acids able to be used comprise citric acid (C6H8O7), formic acid (CH2O2), acetic acid (CH3COOH), sulfamic acid (H3NSO3). Examples of inorganic acids are hydrochloric acid (HCl), nitric acid (HNO3), sulfuric acid (H2SO4), phosphoric acid (H3PO4).

In one advantageous embodiment, at the washing step c) a volume ratio of polar solvent/composition is between 10:90 and 90:10, preferably between 20:80 and 80:20, more preferably between 30:70 and 70:30, further preferably between 40:60 and 60:40.

In one advantageous embodiment, the washing step c) is implemented at a temperature of between 0 °C and 120 °C, preferably between 10 °C and 90 °C, more preferably at ambient temperature.

Preferably, the washing step c) is implemented at a pressure of between 1 bar and 50 bar, more preferably between 1 bar and 30 bar, further preferably between 1 bar and 10 bar, still further preferably at atmospheric pressure.

The washing step c) is performed for example by agitating the product resulting from step a) or b) and the washing solvent in one same vessel, or by counter-current circulation. The duration of step c) is preferably at least 1 mn, more preferably between 1 mn and 10 mn.

Advantageously, the washing step is repeated several times, for example two or three times, with the same or different solvents.

Steps a) to c) allow a significant decrease in the content of silicon and/or chlorine in the composition comprising liquefied-plastic oil. In particular, according to numerous experimental results, the silicon content in the composition obtained after step c) is less than 2 ppm by mass, for an initial value of between 9 ppm and 150 ppm.

In one embodiment, before the mixing step d), the product obtained after the washing step c) is subjected to an additional drying step over an adsorbent such as Na2SO4 and/or distillation and/or any other means for extracting free water.

At the mixing step d), the product obtained after the washing step c) is mixed with a petroleum product comprising at least one petroleum fraction i.e. at least one petroleum distillation fraction. Preferably, the petroleum product is composed of one or more petroleum distillation fractions.

Said one or more petroleum distillation fractions are preferably chosen from among the following fractions or mixtures of fractions, characterized by their initial and final distillation temperatures. Said temperatures, given by way of indication, correspond to distillation at atmospheric pressure:

    • a naphtha/gasoline fraction, having an initial distillation temperature lower than 45 °C and final distillation temperature between 145 °C and 180 °C;
    • a naphtha/gasoline-GPL fraction, comprising a naphtha fraction as defined above and additionally comprising C 3 and C4 alkanes of propane and butane type;
    • a kerosene fraction having an initial distillation temperature of between 145 °C and 180 °C and final distillation temperature of between 240 °C and 300 °C;
    • a gasoil fraction having an initial distillation temperature of between 225 °C and 250 °C and final distillation temperature of between 360 °C and 380 °C;
    • a mixed kerosene-gasoil fraction having an initial distillation temperature of between 145 °C and 180 °C and a final distillation temperature of between 360 °C and 380 °C;
    • an atmospheric residue grouping together the distillation products at temperatures higher than or equal to 360 °C.

Preferably, the petroleum product added at step d) solely comprises one of the fractions or mixtures of fractions described above, and not several of these fractions or mixtures of fractions.

In one advantageous embodiment, the product obtained after step c) undergoes a distillation step f) before being mixed at step d) with a petroleum product. The distillation step f) is conducted with initial and final distillation temperatures close to the initial and final distillation temperatures of the petroleum product at step d). Preferably the initial and final distillation temperatures at step f) are equal to the initial and final distillation temperatures of the petroleum product.

The mixture formed at step d) comprises between 1% by mass and 98% by mass of the product from the preceding step i.e. step c) or f).

The mass percentage of product obtained at said step c) or f) in the mixture obtained at step d) is preferably at least 3%, more preferably at least 5%, further preferably at least 10%, still further preferably at least 15% and most preferably at least 20%.

If the product of step c) has not been subjected to the distillation step f) before being mixed with the petroleum product, said distillation can be performed on the mixture of step d) before implementing step e).

As will be described below, the implementation characteristics of the catalytic hydrotreatment step preferably depend upon the characteristics of the petroleum product added at step d), in particular the initial and final distillation temperatures thereof.

Step e) is a hydrotreatment or hydrorefining step of the mixture obtained at the preceding step. The hydrotreatment step e) is a catalytic treatment step in the presence of hydrogen or dihydrogen (H2) of the mixture obtained at step d), said mixture optionally having been distilled as indicated above.

More specifically, step e) is a hydrotreatment step intended to remove all or some of the sulfur-, nitrogen-, oxygen-containing compounds, and other impurities contained in the mixture obtained at step d). Hydrotreatment inter alia comprises hydrodesulfurization (HDS), hydrodenitrogenation (HDN), hydrodeoxygenation (HDO), hydrogenation (HYD), hydrodearomatization or hydrodemetallization (HDM) reactions.

The hydrotreatment step e) is preferably conducted in a reactor, as is considered in the description given below.

The hydrotreatment catalysts used are preferably supported catalysts comprising an oxide support and at least one hydrogenating function. Said catalysts are known in the prior art.

Preferably, these catalysts can be catalysts containing at least one element in group VIB (Cr, Mo, W) and/or an element in group VIII (Fe, Ru, Os, Co, Rh, Ir, Pd, Ni, Pt). More preferably, these catalysts are catalysts or sulfur-containing type containing at least one element in group VIB (Cr, Mo, W) and/or an element in group VIII (Fe, Co, Ni).

Preferably, the catalyst at step e) comprises a catalyst of sulfur-containing type comprising cobalt-molybdenum CoMo and/or nickel-molybdenum NiMo and/or NiW, or a mixture of these catalysts.

The oxide support is chosen for example from the group formed by alumina, silica, silica-aluminas, zirconium, titanium oxide, clays and mixtures of at least two of these minerals. Advantageously, this support may contain other dopant compounds such as boron, phosphorus or a mixture of these dopants.

Preferably, step e) is conducted under heat and/or pressure. In particular, step e) is conducted at a temperature of between 200 °C and 450 °C, preferably between 250 and 420 °C, more preferably between 250 °C and 400 °C; and at an absolute pressure of between 5 and 200 bar, preferably between 5 and 80 bar, more preferably between 20 and 60 bar.

The liquid hourly space velocity (LHSV), defined as the ratio of volume flow rate of liquid hydrocarbon feed to the total volume of catalyst, can be between 0.5 and 5 h−1, preferably 1 to 4 h−1. The quantity of hydrogen mixed with the feed, defined as the ratio of the volume flow of hydrogen measured under normal conditions of temperature and pressure to the volume flow of liquid hydrocarbon feed, can be between 100 and 1600 Nm3/m3, preferably between 100 and 800 Nm3/m3, more preferably between 200 and 600 Nm3/m3.

For example, step e) is conducted in a fixed bed reactor comprising one or more catalytic beds, each bed comprising at least one hydrotreatment catalyst. The reactor is fed with a flow of the mixture obtained at step d), and with a hydrogen-rich gas flow, in similar manner to the hydrodesulfurization step described in document WO2014/096704.

Optionally, one or more steps or pretreatment sections can be applied upstream of hydrodesulfurization (HDS). This or these pre-treatment steps, called hydrodemetallization steps (HDM), are intended to remove most of the metals in the feed or other impurities, using one or more hydrodemetallization catalysts. For this purpose, a succession of catalysts of different porosity between the HDM section and HDS section can be used, allowing optimized accessibility, at each step, of the active phase, of porosity and of active phase content in similar manner to the description given in document US2006/0060509 for example. In this case, the HDM catalysts used are preferably catalysts known to skilled persons. They generally comprise a metal component from group VIB, preferably molybdenum, on a porous oxide support, generally alumina used alone or in a mixture with other oxides such as silicon, titanium or zirconium. The catalyst may or may not also contain a metal component of group VIII, preferably nickel and/or cobalt, for reasons of economy and performance, preferably nickel. The hydrodemetallization catalyst may contain limited quantities of other ingredients known to skilled persons such as phosphorus, boron, the components of alkali metals and components of alkaline-earth metals. The porosity of the support of the catalysts under consideration can then either be a medium or large pore-size distribution, or a bimodal pore-size distribution combining mesopores allowing maximization of surface area and macropores allowing the diffusion of large molecules, as described in U.S. Pat. No. 7,119,045 or EP1060794.

As a variant, demetallization reactions in the presence of hydrogen are conducted in separate reactors, before the hydrotreatment step e).

Preferably, the implementation characteristics of the catalytic hydrotreatment step e) are dependent on the characteristics of the petroleum product added at step d). In particular, step e) is preferably conducted in known catalytic hydrotreatment units intended for the refining of specific petroleum fractions or specific mixtures such as naphtha/gasoline, naphtha/gasoline-GPL, kerosene, gasoil, kerosene-gasoil fractions and atmospheric residue described above.

It is therefore preferable that the petroleum product added at step d) only contains one of these fractions or mixtures of fractions. Similarly, it is preferable that the composition mixed at step d) with said petroleum product should previously have been subjected to the distillation step f), or alternatively the mixture obtained at step d) should be distilled before step e) at suitable initial and final distillation temperatures.

The low content of silicon and chlorine in the product obtained at c) allows the mixing at step d) to be performed with a high proportion of liquefied-plastic oil, without impacting the hydrotreatment catalyst(s) at step e).

The product obtained after step e) is intended to be used as fuel. In one embodiment, said product of step e) is then subjected to additivation appropriate for said use as fuel. Additives such as corrosion inhibitors, antioxidants, defoaming agents, de-emulsifiers and/or chelators for example are added to the product of step e).

The above-described method therefore allows efficient recycling of liquefied-plastic oils inter alia as waste-to-fuel.

EXAMPLES OF EMBODIMENT OF THE INVENTION

The embodiments of the present invention are illustrated by the following nonlimiting examples.

Example 1: Calculation of a Minimum Quantity of Strong Base to be Contacted with the Composition of Liquefied-Plastic Oil at Step a)

A minimum quantity of strong base to be used at step a) can in particular be estimated as follows:

Let a be the mass percent of oxygen, and b, c and d the respective contents in parts per million of nitrogen, chlorine and silicon, in the composition to be treated.

Let A, B, C and D be the respective molar masses of oxygen, nitrogen, chorine and silicon.

Let M be the molar mass of the strong base to be used (about 40 g/mol for sodium hydroxide) and m a percentage related to the consumption of strong base.

This last value is calculated as follows:

m = [ a A + ( b B + c C + d D ) · 10 - 4 ] × M

Starting from the principle that not all the heteroatoms react with the strong base, as can be the case with carboxylic acid which will consume one equivalent of base per two oxygen atoms, the minimum mass concentration of base a is calculated as follows:


α=∈×m

    • where ∈ is a factor equal to at least 0.5.

Example 2: Purification of Plastic-Pyrolysis Oil in the Presence of a Strong Base and Water, Followed by Washing with Water

The physicochemical characteristics of the plastic-pyrolysis oil used are given in Table 1 below:

TABLE 1 Pyrolysis oil HPP4 Density (g/mL) 0.826 Kinematic viscosity (15 °C, mm2/s) 2.78 Distillation, initial boiling point (°C) 84 Distillation, 50% (°C) 233 Distillation, final boiling point (°C) 398 Silicon (ppm by mass) 45 Chlorine (ppm by mass) 164 Oxygen (% by mass) 1.69 Nitrogen (ppm weight) 3510

Protocol for Tests:

An autoclave in stainless steel of grade AISI-316L, of 1.5 L capacity equipped with mechanical stirring is charged with pyrolysis oil HPP4, a strong base in the form of NaOH and water, the strong base being solubilised in water before being added to the autoclave (Table 2). The sum of the added volume of pyrolysis oil and volume of water is about 600 mL at ambient temperature, without taking into account possible effects of variation in volume at the time of mixing. The autoclave is closed and the gas overhead in the autoclave is flushed with nitrogen for 30 minutes. The autoclave is then heated under autogenous pressure under stirring at a speed of 400 to 1500 rpm and at a temperature of 225 °C for a time of 30 minutes, once the target temperature has been reached. The rate of temperature rise is set at 30 °C/10 minutes.

TABLE 2 Test 1 Pyrolysis oil HPP4 Water/feed volume ratio 0.025 Temperature (°C) 225 Time (min) 30 Volume of water (mL) 14.5 NaOH mass (g) 14.5 Pyrolysis oil mass (g) 481 Initial volume of pyrolysis oil (mL) 584 NaOH concentration in pyrolysis oil 3 (% m/m) NaOH concentration in water (% m/m) 50 Initial density (g/mL) 0.824 Final pressure in autoclave (bar) 13

After the reaction, the autoclave is cooled to ambient temperature and the mixture is discharged and washed three times in water with a water/feed volume ratio for each wash of 40:60, to remove the residues of strong base and water-soluble impurities. The resulting purified and washed pyrolysis oil is analysed to measure the content of residual impurities (Table 3).

TABLE 3 Test 1 Initial silicon (ppm weight) 45 Final silicon (ppm weight) <2 Silicon removal (%) >95 Initial chlorine (ppm weight) 164 Final chlorine (ppm weight) 16 Chlorine removal (%) 90 Initial oxygen (wt. %) 1.69 Final oxygen (wt. %) 0.38 Oxygen removal (%) 78 Initial nitrogen (ppm weight) 3510 Final nitrogen (ppm weight) 881 Nitrogen removal (%) 75 Initial sodium (ppm weight) <2 Final sodium (ppm weight) <2

The data in Table 3 show that the use of sodium hydroxide in the presence of water followed by washing allows a major decrease in the impurities initially contained in the pyrolysis oil, and the sodium added by treatment with sodium hydroxide.

The pyrolysis oil is either used as such, or optionally dried over an adsorbent such as a molecular sieve or anhydrous salt e.g. Na2SO4, then distilled under reduced pressure to remove any possible trace of solid e.g. of strong base, or adsorbent residue, anhydrous/hydrated salt or gums.

Example 3: Mixing of the Product of Example 2 with a Petroleum Product

A petroleum product of SRGO type is considered (Straight Run Gas Oil) having the following characteristics (Table 4):

TABLE 4 OPE 7028 Density (g/mL) 0.8575 ASTM D86 - T5% (°C) 255 ASTM D86 - T95% (°C) 370 Total nitrogen (ppm by mass) 160 Sulfur (ppm by mass) 11000

It is considered that the contents of silicon and chlorine of the SRGO are negligible.

The mixtures given below are considered of said SRGO with the product of step 2 (treated HPP4) or with the initial non-treated HPP4 (HPP4), according to the silicon and chlorine contents thereof (Table 5). The mixtures are expressed as weight percent of HPP4 treated or non-treated. The column “HDS specification” corresponds to the maximum permissible values of silicon and chlorine content in a product before being treated in an industrial catalytic hydrodesulfurization reactor:

TABLE 5 HDS SRGO + SRGO + SRGO + SRGO + Contents Specifi- 2% 2% treated 10% 10% treated (ppm) cation HPP4 HPP4 HPP4 HPP4 Si <1 0.9 <<1    4.5 <<1    Cl <2 3.3 0.3 16.4 1.6

The treatment method of the HPP4 oil of the invention allows this oil to be added in an amount of 10% by mass in a mixture with SRGO, while meeting the requirements for the catalytic hydrodesulfurization step.

On the contrary, without the treatment of the invention, the mixture with 10% HPP4 exceeds silicon and chorine specifications, and the mixture with 2% HPP4 exceeds the specifications for chlorine.

With the treatment method of the invention, it is therefore possible to increase the quantity of oil derived from plastic recycling in mixtures with petroleum products, intended in particular for the production of fuels.

Claims

1. A method for treating a composition comprising a liquefied-plastic oil, said composition comprising at least 5 ppm by mass of silicon as measured according to standard ISO20884, and/or at least 2 ppm by mass of chlorine as measured according to standard ASTM D7359, said treatment-method comprising:

a) a contacting step, under heat, of said composition with a strong base; then
c) a washing step with a polar solvent immiscible with the product obtained in the preceding step, said solvent being chosen from water, an organic polar solvent and mixtures thereof; then
d) a mixing step of the product from the preceding step with a petroleum product comprising at least one petroleum distillation fraction, the mixture obtained comprising between 1% by mass and 98-% by mass of the product from the preceding step; then
e) a catalytic hydrotreatment step, in the presence of hydrogen, of the mixture obtained at the preceding step.

2. The method according to claim 1, wherein the strong base at step a) comprises an oxide, a hydroxide, a bicarbonate or alcoholate of an alkali metal cation or alkaline-earth metal cation, or a hydroxide or a bicarbonate of a quaternary ammonium cation, alone or in a mixture.

3. The method according to claim 1 comprising, before step c), a separation step b) to separate the composition from the strong base.

4. The treatment method according to claim 1, wherein the polar solvent at step c) is water at neutral or acid pH.

5. The method according to claim 1, wherein step a) is performed in the presence of water, preferably in the presence of a concentrated aqueous solution of the strong base, more preferably in the presence of a saturated aqueous solution of the strong base.

6. The method according to claim 1, wherein step a) is performed in the presence of an organic polar solvent comprising an alcohol function and/or ether function.

7. The according to claim 1, wherein the strong base at step a) is in solid form.

8. The method according to claim 1, wherein step a) is conducted at a temperature of at least 85 °C, preferably at least 100 °C, more preferably at least 150 °C, further preferably at least 180 °C.

9. The method according to claim 1, wherein: the petroleum product at the mixing step d) is characterized by initial and final distillation temperatures; and before the mixing step d), the product obtained at step c) is subjected to a distillation step f) with initial and final distillation temperatures similar to the initial and final distillation temperatures of said petroleum product.

10. The method according to claim 1, wherein the mixture obtained at step d) comprises at least 3% by mass, preferably at least 5% by mass, more preferably at least 10% by mass, further preferably at least 15% by mass, and still further preferably at least 20% by mass of the product obtained at the preceding step.

11. The method according to claim 1, wherein the comprising a liquefied-plastic oil additionally comprises a biomass oil.

12. The method according to claim 1, next comprising a step to add additives to the product obtained at the catalytic hydrotreatment step e), such that said product is made suitable for use as fuel.

Patent History
Publication number: 20260337501
Type: Application
Filed: Oct 25, 2023
Publication Date: Oct 29, 2026
Applicant: TotalEnergies OneTech (COURBEVOIE)
Inventors: Thomas COUSTHAM (SOLAIZE), Cindy ADAM (SOLAIZE), Delphine MINOUX (SOLAIZE), Hélène COULOMBEAU-LEROY (SOLAIZE), Anne VILBE (SOLAIZE)
Application Number: 19/123,312
Classifications
International Classification: C10G 67/10 (20060101);