Preparation Method for Non-magnetic Low-expansion Chromium-based Alloy Material
A treatment method for non-magnetic low-expansion chromium-based alloy material comprises steps of: designing material composition; preparing raw materials; powder mixing; powder molding; sintering; and post-treatment. The chromium-based alloy itself has low magnetic conductivity, and the low-temperature thermal expansion coefficient of the chromium-based alloy is reduced by adding the phosphorus. By controlling the contents of iron, phosphorus and manganese, the thermal expansion coefficient of the chromium-based alloy can be regulated in a certain range. By directly using press sintering, metal injection molding or other powder metallurgy processes, a small number of pores unique to powder metallurgy processes are also beneficial for the reduction of the thermal expansion coefficient. The treatment method of the present invention has the advantages of simple preparation process, low cost, high material utilization, few machining steps, improved production efficiency, and can be used for high-precision electronic devices and instruments.
The present invention relates to a field of powder metallurgy, and in particular to a treatment method for non-magnetic low-expansion chromium-based alloy material.
BACKGROUND OF THE INVENTIONIn many electronic devices and precise instruments and devices, it is often needed to seal or couple an alloy with a low expansion coefficient with other ceramic or glass parts. Mismatched thermal expansion will lead to the damage or failure of devices. Non-magnetic low-expansion stainless alloys are special materials used in many key components of these electronic instruments. Particularly in high-precision modern electronic instruments, expansion alloys are required to have near-vacuum non-magnetic properties in addition to low expansion coefficient, ensuring the anti-interference performance, reliability and high precision of the devices. Since a micro magnetic field will lead to serious attenuation, signal drift and precision decline of instruments, such materials are stipulated to have a magnetic conductivity of u=1-1.0003.
At present, there are three main ways to obtain sealing alloys with a certain thermal expansion coefficient: the first way is to realize low expansion on the basis of the Curie transition temperature, for example, ferromagnetic invar alloys of Fe—Ni and Fe—Co—Cr series; the second way is to obtain Mn-based or Cr-based non-magnetic invar alloys with low expansion coefficients on the basis of the Nair transition temperature; and, the third way is to adjust alloy elements to satisfy the desired non-magnetic low-expansion properties by using the lever distribution rule for the thermal expansion coefficient of the refractory metal based alloy in the solid solution and multiphase mixture.
On one hand, it is expected to develop non-magnetic low-expansion alloys on the basis of Fe—Ni and Fe—Co—Cr invar alloys and replace Fe and Ni with numerous low-expansion paramagnetic refractory metal elements to obtain the non-magnetic low-expansion performance; on the other hand, it is attempted to expand the use temperature range of the Mn base and the Cr base so as to improve the machinability.
As refractory high-temperature alloys, chromium-based alloys have lower thermal expansion coefficients and better oxidation resistance than ordinary iron-based alloys and nickel-based alloys. However, the chromium-based alloy materials are brittle and poor in machinability, so it is difficult to manufacture the chromium-based alloy materials into low-expansion components. Therefore, it is necessary to develop a treatment method for a non-magnetic low-expansion chromium-based alloy material.
SUMMARY OF THE INVENTIONIt is an object of the present invention to provide a treatment method for non-magnetic low-expansion chromium-based alloy material.
For achieving the above object, the treatment method comprises steps of:
-
- 1) designing material composition: the used material is a chromium-based alloy, and the mass percentage of each component is as follows: 0% to 10% of iron, more than 0% to 2% of phosphorus, ≤0.2% of silicon, ≤0.2% of aluminum, 0.2% to 1.5% of manganese, no more than 2% of inevitable impurities, and the rest of chromium;
- 2) preparing raw materials: pure chromium powder, pure iron powder, phosphorus iron powder, manganese iron alloy powder and a lubricant;
- 3) powder mixing: weighing the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and 0.1% to 1% of the lubricant from the material composition designed in the step-1, successively adding the weighed powder into a mixer, and uniformly mixing the weighed powder to obtain powder to be pressed;
- 4) powder molding: pressing and molding the powder to be pressed at a pressing pressure of 400 to 1200 MPa to obtain a blank with a specified shape and size;
- 5) sintering: placing the blank on a bearing plate, and then placing the blank into a sintering furnace for sintering for 10 min to 240 min at a sintering temperature of 1350 °C to 1700 °C; and
- 6) post-treatment: for some parts that cannot be formed by molding, a machining step is adopted to obtain the desired shape and size; and/or, for parts with air tightness requirements, a process of pore sealing by oxidation is adopted; and/or, for parts with high electrical conductivity requirements, the surface of the parts can be plated with copper, or silver, or copper and then silver, or post-treatment is not needed. In other words, the post-treatment selectively uses the corresponding treatment process as required, and is not a necessary step.
Preferably, the pure chromium powder in the step-2 comprises the following main components by mass percentage: ≤0.5% of iron, ≤0.2% of silicon, ≤0.2% of aluminum, no more than 2% of inevitable impurities, and the rest of chromium; and, the selected particle size of the powder is 13 μm to 250 μm.
Preferably, the pure iron powder in the step-2 comprises atomized iron powder, reduced iron powder and carbonyl iron power; the pure iron powder comprises the following main components by mass percentage: ≤0.2% of silicon, ≤0.2% of aluminum, ≤0.03% of carbon, no more than 2% of inevitable impurities, and the rest of iron; and, the selected particle size of the powder is 13 μm to 250 μm.
Preferably, the phosphorus iron powder in the step-2 comprises the following main components by mass percentage: 15% to 23% of phosphorus, ≤0.4% of carbon, ≤1.0% of silicon, ≤1.0% of manganese, ≤0.1% of sulfur, and the rest of iron; and, the particle size of the powder is 1 μm to 150 μm.
Preferably, the manganese iron alloy powder in the step-2 comprises the following main components by mass percentage: 10% to 94% of manganese, ≤0.2% of carbon, ≤1.0% of silicon, ≤0.1% of sulfur, and the rest of iron; and, the particle size of the powder is 1 μm to 150 μm.
Preferably, the lubricant in the step-2 is an amide-based, paraffin-based or stearate powdery lubricant.
Preferably, the raw materials in the step-2 are not limited to the pure iron powder and can also be added in the form of chromium iron alloy powder, and the chromium iron alloy powder has a particle size of 13 μm to 250 μm.
Preferably, the raw materials in the step-2 are not limited to the manganese iron alloy powder, and can also be added as the manganese source in the step-1 in the form of pure metal manganese powder such as electrolytic manganese powder, and the metal manganese powder has a particle size of 3 μm to 250 μm.
Preferably, during the powder molding in the step-4, during the molding of a part with complex shape or thin wall, the blank can be molded by metal injection molding; and correspondingly, the particle size of the pure chromium powder, the pure iron powder, the manganese iron alloy powder and the phosphorus iron powder in the step-2 is ≤500 meshes.
Finally, the sintering furnace in the step-5 is a batch-type vacuum sintering furnace or a continuous sintering furnace, for the vacuum sintering furnace, the vacuum degree is 10−5 Pa to 102 Pa, and argon at 102 Pa to 5*104 Pa can be back-flushed near the sintering holding temperature, and, for the continuous sintering furnace, the sintering atmosphere is pure hydrogen or pure argon or a mixed gas of hydrogen and argon.
Compared with the prior art, the treatment method for non-magnetic low-expansion chromium-based alloy material of the present invention has the following advantages. The material composition is designed scientifically and reasonably. The chromium-based alloy itself has low magnetic conductivity, and the low-temperature thermal expansion coefficient of the chromium-based alloy is reduced by adding the phosphorus. By controlling the contents of iron, phosphorus and manganese, the thermal expansion coefficient of the chromium-based alloy is regulated in a certain range. By directly using press sintering, metal injection molding or other powder metallurgy processes, a small number of pores unique to powder metallurgy processes are also beneficial for the reduction of the thermal expansion coefficient. The treatment method of the present invention has the advantages of simple preparation process, low cost, high material utilization, few machining steps and improved production efficiency. Moreover, the treated chromium-based alloy material is non-magnetic and low in expansion, and can be used for high-precision electronic devices and instruments.
The present invention will be further described below in detail by embodiments with reference to the accompanying drawings.
Embodiment 1Step-1, design of material composition: the chromium-based alloy comprises the following components by mass percentage: 5.0% of Fe, 0.8% of P, ≤0.2% of Si, ≤0.2% of Al, 0.5% of Mn, no more than 2.0% of inevitable impurities, and the rest of Cr.
Step-2, preparation of raw materials:
-
- pure chromium powder: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of Al, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes (particles passing through a 100-mesh sieve), and inevitable impurities. The microscopic morphological view of the pure chromium powder is shown in
FIG. 1 ; - pure iron powder: 99.40% of Fe, 0.25% of Mn, 0.03% of Si, 0.01% of C, 0.015% of S, 0.015% of P, 0.07% of O, and 0.05% of Al, with a particle size of −100 meshes, and inevitable impurities. The microscopic morphological view of the pure iron powder is shown in
FIG. 2 . - phosphorus iron powder: 81.6% of Fe, 18.0% of P, 0.05% of C, 0.03% of Si, 0.30% of Mn, and 0.02% of S, with a particle size D50=12 μm. The microscopic morphological view of the phosphorus iron powder is shown in
FIG. 3 ; - manganese iron alloy powder: 90% of Mn, 0.05% of C, 0.56% of Si, 0.02% of S, and the rest of Fe, with a particle size D50=20 μm;
- lubricant: an amide-based powdery lubricant is selected and added in a mass percentage of 0.8%.
- pure chromium powder: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of Al, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes (particles passing through a 100-mesh sieve), and inevitable impurities. The microscopic morphological view of the pure chromium powder is shown in
Step-3, powder mixing: the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and the lubricant are weighed by the designed mass percentage, and the weighed powder is successively added into a mixer and then uniformly mixed to obtain powder to be pressed.
Step-4, powder molding: the powder to be pressed is pressed and molded at a pressing pressure of 700 MPa to obtain a blank with a specified shape and size.
Step-5, sintering: the blank is placed on a bearing plate, and then placed into a vacuum sintering furnace for sintering for 180 min at a sintering temperature of 1550 °C. The vacuum degree of the vacuum sintering surface is 10−5 Pa to 102 Pa. To prevent the evaporation of chromium and other elements, argon with 3*104 Pa is back-flushed near the sintering holding temperature. The metallographic view of the sintered part is shown in
Step-1, design of material composition: the chromium-based alloy comprises the following components by mass percentage: 4.0% of Fe, 0.6% of P, ≤0.2% of Si, ≤0.2% of Al, 1.0% of Mn, no more than 2.0% of inevitable impurities, and the rest of Cr.
Step-2, preparation of raw materials:
-
- pure chromium powder: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of Al, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes, and inevitable impurities;
- pure iron powder: 99.40% of Fe, 0.25% of Mn, 0.03% of Si, 0.01% of C, 0.015% of S, 0.015% of P, 0.07% of O, and 0.05% of Al, with a particle size of −100 meshes, and inevitable impurities;
- phosphorus iron powder: 81.6% of Fe, 18% of P, 0.05% of C, 0.03% of Si, 0.30% of Mn, and 0.02% of S, with a particle size D50=12 μm;
- manganese iron alloy powder: 80% of Mn, 0.07% of C, 0.32% of Si, 0.01% of S, and the rest of Fe, with a particle size D50=10 μm;
- lubricant: an amide-based powdery lubricant is selected and added in a mass percentage of 1%.
Step-3, powder mixing: the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and the lubricant are weighed by the designed mass percentage, and the weighed powder is successively added into a mixer and then uniformly mixed to obtain powder to be pressed.
Step-4, powder molding: the powder to be pressed is pressed and molded at a pressing pressure of 800 MPa to obtain a blank with a specified shape and size.
Step-5, sintering: the blank is placed on a bearing plate, and then placed into a vacuum sintering furnace for sintering for 240 min at a sintering temperature of 1500 °C. The vacuum degree of the vacuum sintering surface is 10−5 Pa to 102 Pa. To prevent the evaporation of chromium and other elements, argon with 2*104 Pa is back-flushed near the sintering holding temperature.
It can be seen that the part had few pores and uniform structure, and has a thermal expansion coefficient of lower than 1*10−6/K below 160 °C.
Embodiment 3Step-1, design of material composition: the chromium-based alloy comprises the following components by mass percentage: 6% of Fe, 1.0% of P, ≤0.2% of Si, ≤0.2% of Al, 0.3% of Mn, no more than 2.0% of inevitable impurities, and the rest of Cr.
Step-2, preparation of raw materials:
-
- pure chromium powder comprises the following components by mass percentage: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of Al, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes, and inevitable impurities;
- pure iron powder: 99.40% of Fe, 0.25% of Mn, 0.03% of Si, 0.01% of C, 0.015% of S, 0.015% of P, 0.07% of O, and 0.05% of Al, with a particle size of −100 meshes, and inevitable impurities;
- phosphorus iron powder: 81.6% of Fe, 18% of P, 0.05% of C, 0.03% of Si, 0.30% of Mn, and 0.02% of S, with a particle size D50=12 μm;
- manganese iron alloy powder: 15% of Mn, 0.15% of C, 0.82% of Si, 0.01% of S, and the rest of Fe, with a particle size D50=30 μm;
- lubricant: an amide-based powdery is selected as the lubricant and added in a mass percentage of 0.6%.
Step-3, powder mixing: the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and the lubricant are weighed by the designed mass percentage, and the weighed powder is successively added into a mixer and then uniformly mixed to obtain powder to be pressed.
Step-4, powder molding: the powder to be pressed is pressed and molded at a pressing pressure of 600 MPa to obtain a blank with a specified shape and size.
Step-5, sintering: the blank is placed on a bearing plate, and then placed into a vacuum sintering furnace for sintering for 120 min at a sintering temperature of 1600 °C. The vacuum degree of the vacuum sintering surface is 10−5 Pa to 102 Pa. To prevent the evaporation of chromium and other elements, argon with 1*104 Pa is back-flushed near the sintering holding temperature.
It can be seen that the part has few pores and uniform structure, and has a thermal expansion coefficient of lower than 1*10−6/K below 160 °C.
Embodiment 4Step-1, design of material composition: the chromium-based alloy comprises the following components by mass percentage: 10% of Fe, 1.0% of P, ≤0.2% of Si, ≤0.2% of Al, 0.3% of Mn, no more than 2% of inevitable impurities, and the rest of Cr.
Step-2, preparation of raw materials:
-
- pure chromium powder: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of Al, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes, and inevitable impurities;
- chromium iron alloy powder: 65% of Cr, 0.03% of C, 0.7% of Si, and the rest of Fe, with a particle size of −100 meshes;
- phosphorus iron powder: 81.6% of Fe, 18% of P, 0.05% of C, 0.03% of Si, 0.30% of Mn, and 0.02% of S, with a particle size D50=12 μm;
- manganese source: electrolytic manganese powder being used as manganese source comprises the following components by mass percentage: 99.6% of Mn, 0.2% of Fe, 0.10% of O, and 0.10% of Si;
- lubricant: an amide-based powdery is selected as the lubricant and added in a mass percentage of 0.6%.
Step-3, powder mixing: the pure chromium powder, the chromium iron alloy powder, the phosphorus iron powder, the electrolytic manganese powder and the lubricant are weighed by the designed mass percentage, and the weighed powder is successively added into a mixer and then uniformly mixed to obtain powder to be pressed.
Step-4, powder molding: the powder to be pressed is pressed and molded at a pressing pressure of 800 MPa to obtain a blank with a specified shape and size.
Step-5, sintering: the blank is placed on a bearing plate, and then placed into a sintering furnace operated by pushing a rod continuously for sintering for 80 min at a sintering temperature of 1480 °C. The sintering atmosphere is pure hydrogen, and nitrogen is used as gas curtain at a head and a tail of the sintering furnace to prevent an air to enter the sintering furnace.
It can be seen that the part has few pores and uniform structure, and has a thermal expansion coefficient of lower than 1*10−6/K below 160 °C.
Embodiment 5Step-1, design of material composition: the chromium-based alloy comprises the following components by mass percentage: 0.825% of Fe, 0.17% of P, ≤0.2% of Si, ≤0.2% of Al, 0.7% of Mn, no more than 2% of inevitable impurities, and the rest of Cr.
Step-2, preparation of raw materials:
-
- pure chromium powder: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of A 1, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes, and inevitable impurities;
- phosphorus iron powder: 77.3% of Fe, 22.2% of P, no more than 0.5% of other components, and inevitable impurities, with a particle size D50=12 μm;
- manganese iron alloy powder: 70% of Mn, 0.08% of C, 0.32% of Si, 0.01% of S, and the rest of Fe, with a particle size D50=8 μm;
- lubricant: a paraffin-based powdery is selected as the lubricant and added in a mass percentage of 0.7%.
Step-3, powder mixing: the pure chromium powder, the phosphorus iron powder, the manganese iron alloy powder and the lubricant are weighed by the designed mass percentage, and the weighed powder is successively added into a mixer and then uniformly mixed to obtain powder to be pressed.
Step-4, powder molding: the powder to be pressed is pressed and molded at a pressing pressure of 800 MPa to obtain a blank with a specified shape and size.
Step-5, sintering: a sintering furnace operated by pushing a rod continuously is used for sintering for 80 min at a sintering temperature of 1480 °C. The sintering atmosphere is pure hydrogen, and nitrogen is used as gas curtain at a head and a tail of the sintering furnace to prevent an air to enter the sintering furnace.
It can be seen that the part has few pores and uniform structure, and has a thermal expansion coefficient of lower than 1*10−6/K below 160 °C.
Embodiment 6Step-1, design of material composition: the chromium-based alloy comprises the following components by mass percentage: 7% of Fe, 0.5% of P, ≤0.2% of Si, ≤0.2% of Al, 1.4% of Mn, no more than 2% of inevitable impurities, and the rest of Cr.
Step-2, preparation of raw materials:
-
- pure chromium powder: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of Al, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes, and inevitable impurities. The microscopic morphological view of the pure chromium powder is shown in
FIG. 1 ; - pure iron powder: 99.40% of Fe, 0.25% of Mn, 0.03% of Si, 0.01% of C, 0.015% of S, 0.015% of P, 0.07% of O, and 0.05% of Al, with a particle size of −100 meshes, and inevitable impurities. The microscopic morphological view of the pure iron powder is shown in
FIG. 2 ; - phosphorus iron powder: 81.6% of Fe, 18% of P, 0.05% of C, 0.03% of Si, 0.30% of Mn, and 0.02% of S, with a particle size D50=12 μm. The microscopic morphological view of the phosphorus iron powder is shown in
FIG. 3 ; - manganese iron alloy powder: 85% of Mn, 0.20% of C, 0.69% of Si, 0.01% of S, and the rest of Fe, with a particle size D50=25 μm;
- lubricant: lithium stearate powdery is selected as the lubricant and added in a mass percentage of 0.8%.
- pure chromium powder: 99.50% of Cr, 0.13% of Fe, 0.08% of Si, 0.07% of Al, 0.006% of C, 0.007% of N, 0.09% of O, and 0.004% of S, with a particle size of −100 meshes, and inevitable impurities. The microscopic morphological view of the pure chromium powder is shown in
Step-3, powder mixing: the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and the lubricant are weighed by the designed mass percentage, and the weighed powder is successively added into a mixer and then uniformly mixed to obtain powder to be pressed.
Step-4, powder molding: the powder to be pressed is pressed and molded at a pressing pressure of 800 MPa to obtain a blank with a specified shape and size.
Step-5, sintering: the blank is placed on a bearing plate, and then placed into a vacuum sintering furnace for sintering for 200 min at a sintering temperature of 1480 °C. The vacuum degree of the vacuum sintering surface is 10−5 Pa to 102 Pa. To prevent the evaporation of chromium and other elements, argon with 4*104 Pa is back-flushed near the sintering holding temperature.
Step-6, post-treatment: the sintered part is oxidized for pore sealing and then grinded to satisfy the shape and size requirements, and the part is plated with copper and then silver to satisfy the electrical conductivity requirements.
It can be seen that the part has few pores and uniform structure, and has a thermal expansion coefficient of lower than 1*10−6/K below 160 °C.
The specific experimental pictures and thermal expansion curve charts of the treatment method according to Embodiment 1 of the present application are shown in Figs, and thermal expansion curve charts in other embodiments are similar to that in Embodiment 1.
The protection scope of the present invention is not limited to each embodiment described in this description. Any changes and replacements made on the basis of the scope of the present invention patent and of the description shall be included in the scope of the present invention patent.
Claims
1. A treatment method for non-magnetic low-expansion chromium-based alloy material, comprising steps of:
- 1) designing material composition: the used material is a chromium-based alloy, and the mass percentage of each component is as follows: 0% to 10% of iron, more than 0% to 2% of phosphorus, ≤0.2% of silicon, ≤0.2% of aluminum, 0.2% to 1.5% of manganese, no more than 2% of inevitable impurities, and the rest of chromium;
- 2) preparing raw materials: pure chromium powder, pure iron powder, phosphorus iron powder, manganese iron alloy powder and a lubricant;
- 3) powder mixing: weighing the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and 0.1% to 1% of the lubricant from the material composition designed in the step 1, successively adding the weighed powder into a mixer, and uniformly mixing the weighed powder to obtain powder to be pressed;
- 4) powder molding: pressing and molding the powder to be pressed at a pressing pressure of 400 to 1200 MPa to obtain a blank with a specified shape and size;
- 5) sintering: placing the blank on a bearing plate, and then placing the blank into a sintering furnace for sintering for 10 min to 240 min at a sintering temperature of 1350 °C to 1700 °C; and
- 6) post-treatment: for some parts that cannot be formed by molding, a machining step is adopted to obtain parts with desired shape and size.
2. The treatment method of claim 1, wherein the pure chromium powder in the step 2 comprises the following main components by mass percentage: ≤0.5% of iron, ≤0.2% of silicon, ≤0.2% of aluminum, no more than 2% of inevitable impurities, and the rest of chromium, and, the selected particle size of the powder is 13 μm to 250 μm.
3. The treatment method of claim 1, wherein the pure iron powder in the step 2 comprises atomized iron powder, reduced iron powder and carbonyl iron power; the pure iron powder comprises the following main components by mass percentage: ≤0.2% of silicon, ≤0.2% of aluminum, ≤0.03% of carbon, no more than 2% of inevitable impurities, and the rest of iron; and, the selected particle size of the powder is 13 μm to 250 μm.
4. The treatment method of claim 1, wherein the phosphorus iron powder in the step 2 comprises the following main components by mass percentage: 15% to 23% of phosphorus, ≤0.4% of carbon, ≤1.0% of silicon, ≤1.0% of manganese, ≤0.1% of sulfur, and the rest of iron; and, the particle size of the powder is 1 μm to 150 μm.
5. The treatment method of claim 1, wherein the manganese iron alloy powder in the step 2 comprises the following main components by mass percentage: 10% to 94% of manganese, ≤0.2% of carbon, ≤1.0% of silicon, ≤0.1% of sulfur, and the rest of iron; and, the particle size of the powder is 1 μm to 150 μm.
6. The treatment method of claim 1, wherein the manganese iron alloy powder in the step 2 can also be added as the manganese source in the form of pure metal manganese powder such as electrolytic manganese powder, and the metal manganese powder has a particle size of 3 μm to 250 μm.
7. The treatment method of claim 1, wherein the lubricant in the step 2 is an amide-based, paraffin-based or stearate powdery lubricant.
8. The treatment method of claim 1, wherein the raw materials in the step 2 are not limited to the pure iron powder and can also be added in the form of chromium iron alloy powder, and the chromium iron alloy powder has a particle size of 13 μm to 250 μm.
9. The treatment method of claim 1, wherein during the powder molding in the step 4, during the molding of a part with complex shape or thin wall, the blank can be molded by metal injection molding, and correspondingly, the particle size of the pure chromium powder, the pure iron powder, the manganese iron alloy powder and the phosphorus iron powder in the step 2 is ≤500 meshes.
10. The treatment method of claim 1, wherein the sintering furnace in the step 5 is a batch-type vacuum sintering furnace or a continuous sintering furnace, for the vacuum sintering furnace, the vacuum degree is 10−5 Pa to 102 Pa, and argon at 102 Pa to 5*104 Pa can be back-flushed near the sintering holding temperature, and, for the continuous sintering furnace, the sintering atmosphere is pure hydrogen or pure argon or a mixed gas of hydrogen and argon.
11. A treatment method for non-magnetic low-expansion chromium-based alloy material, comprising steps of:
- 1) designing material composition: the used material is a chromium-based alloy, and the mass percentage of each component is as follows: 0% to 10% of iron, more than 0% to 2% of phosphorus, ≤0.2% of silicon, ≤0.2% of aluminum, 0.2% to 1.5% of manganese, no more than 2% of inevitable impurities, and the rest of chromium;
- 2) preparing raw materials: pure chromium powder, pure iron powder, phosphorus iron powder, manganese iron alloy powder and a lubricant;
- 3) powder mixing: weighing the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and 0.1% to 1% of the lubricant from the material composition designed in the step 1, successively adding the weighed powder into a mixer, and uniformly mixing the weighed powder to obtain powder to be pressed;
- 4) powder molding: pressing and molding the powder to be pressed at a pressing pressure of 400 to 1200 MPa to obtain a blank with specified shape and size;
- 5) sintering: placing the blank on a bearing plate, and then placing the blank into a sintering furnace for sintering for 10 min to 240 min at a sintering temperature of 1350 °C to 1700 °C.
12. The treatment method of claim 1, wherein in the post-treatment, for parts with air tightness requirements, a process of pore sealing by oxidation is adopted.
13. The treatment method of claim 1, wherein in the post-treatment, for parts with high electrical conductivity requirements, the surface of the parts can be plated with copper, or silver, or copper and then silver.
14. A treatment method for non-magnetic low-expansion chromium-based alloy material, comprising steps of:
- 1) designing material composition: the used material is a chromium-based alloy, and the mass percentage of each component is as follows: 0% to 10% of iron, more than 0% to 2% of phosphorus, ≤0.2% of silicon, ≤0.2% of aluminum, 0.2% to 1.5% of manganese, no more than 2% of inevitable impurities, and the rest of chromium;
- 2) preparing raw materials: pure chromium powder, pure iron powder, phosphorus iron powder, manganese iron alloy powder and a lubricant;
- 3) powder mixing: weighing the pure chromium powder, the pure iron powder, the phosphorus iron powder, the manganese iron alloy powder and 0.1% to 1% of the lubricant from the material composition designed in the step 1, successively adding the weighed powder into a mixer, and uniformly mixing the weighed powder to obtain powder to be pressed;
- 4) powder molding: pressing and molding the powder to be pressed at a pressing pressure of 400 to 1200 MPa to obtain a blank with a specified shape and size;
- 5) sintering: placing the blank on a bearing plate, and then placing the blank into a sintering furnace for sintering for 10 min to 240 min at a sintering temperature of 1350 °C to 1700 °C.
Type: Application
Filed: Oct 14, 2022
Publication Date: Nov 5, 2026
Inventors: Chongxi Bao (Ningbo), Zhidong Chen (Ningbo), Weiwei Yan (Ningbo), Zhirong Zhu (Ningbo)
Application Number: 18/997,566