RANDOMLY BONDED POLYSACCHARIDE CONTAINING FIBROUS STRUCTURES WITH IMPROVED SURFACE PROPERTIES

Fibrous structures having improved properties, including surface smoothness, smooth layer for softener deposition, low lint, and good wet feel.

Skip to: Description  ·  Claims  · Patent History  ·  Patent History
Description
FIELD OF THE INVENTION

The present invention relates to fibrous structures and more particularly to fibrous structures that exhibit improved properties, for example surface smoothness, smooth layer for softener deposition, low lint, good wet feel, compared to known fibrous structures.

BACKGROUND OF THE INVENTION

Consumer desirable product characteristics in a cellulosic tissue product, such as balancing softness, strength, and absorbency properties, are delivered to the tissue in the papermaking and converting processes. However, it is often observed that structural or process transformations that improve one desirable attribute have the unintended consequence of degrading another desirable attribute. Consequently, designing tissue products with the right combination of product benefits can be very challenging for formulators.

It is well known that a nonwoven layer of polyvinyl alcohol (PVOH) melt blown onto a wet laid substrate delivers a mobile surface layer that provides glide and comfort while creating a smooth, flat surface for uniform application of surface softeners further driving consumer preference. This is accomplished through a discrete bonding process, such as a thermal bonding process that bonds the spun filament layer onto the wet laid structure surface. The bonding process is required to keep the spun filaments in place on the wet laid structure surface during web processing or in-use; poorly bonded spun filaments can lead to processing issues or undesirable use issues like pilling and lint. The problem with this approach is that while a thermal bonding process does affix the spun filaments, it deteriorates the filament surface layer mobility resulting in decreased softness and flexibility.

Thus, there is a need to sufficiently attach a spun filament surface layer to wet laid paper without the use of thermal bonding or other discrete bonding methods.

SUMMARY OF THE INVENTION

The present invention fulfills the need described above by providing a layered fibrous structure, for example a surface layer of spun hydroxyl polymer filaments on a wet laid cellulosic substrate where the spun filaments are attached to the wet laid fibrous structure without the use of thermal bonding or other discrete bonding methods. The resulting fibrous structures have improved softness without the negatives associated with known fibrous structures with no discrete bonding such as high lint and high pilling. One solution to the problem described above is to melt blow a layer of hydroxyl polymer filaments onto a wet laid cellulosic substate by 1) decreasing the degree of drying of the hydroxyl polymer filaments before they are applied to the wet laid substrate and 2) passing a high volumetric flowrate of forming air through the spun fiber layer/wet laid cellulose structure. This results in a forming zone of high humidity and high forming vacuum. The former increases the moisture content of the spun fiber at laydown thereby decreasing its storage modulus (G′) and the later ensures there is sufficient force between the hydroxyl polymer filament layer and wet laid cellulosic structure to staple and securely attach the layers together. The resulting layered substrate has a structure with new degrees of fiber mobility and new combinations of softness and low lint and low pilling.

A fibrous structure is provided that comprises a first web material and a consumer facing outer surface comprising a surface material different from the first web material, wherein the surface material comprises a polysaccharide fiber composition bonded to the first web material, wherein the fibrous structure has a pilling less than 10,000 mm3.

BRIEF DESCRIPTION OF THE DRAWINGS

Many aspects of this disclosure can be better understood with reference to the following figures, which illustrate examples according to various embodiments.

FIG. 1A is an SEM cross-sectional view of a thermally bonded PVOH layer.

FIG. 1B is an SEM cross-sectional view of a non-thermal bonded layer.

FIG. 2 is a schematic representation of an example of a fibrous structure according to the present invention.

FIG. 3 is a cross-sectional view of FIG. 1 taken along line 2-2.

FIG. 4 is a schematic cross-sectional representation of an example of a multi-ply fibrous structure according to the present invention.

FIG. 5 is a schematic cross-sectional representation of another example of a fibrous structure according to the present invention.

FIG. 6 is a schematic representation of a process for making a fibrous structure according to the present invention.

FIG. 7 is a schematic partial top view representation of a surface material source used in the process shown in FIG. 5.

FIG. 8 is a schematic representation of an example of a through-air-drying papermaking process for making a first web material according to the present invention.

FIG. 9 shows the parameters for the Surface Topography Test Method.

FIG. 10 is an illustration of the Ply Bond Test Method.

FIG. 11 is an illustration of the Ply Bond Test Method.

FIG. 12 is an illustration of the Ply Bond Test Method.

FIG. 13 shows optical profilometry results of a base wet laid substrate, a PVOH layer thermal bonded to a wet laid substrate (comparative example), and a PVOH layer randomly bonded to a wet laid substrate (inventive example).

FIG. 14 is a graph showing how G′ varies for PVOH filaments with both relative humidity (RH) and temperature.

FIG. 15 is a schematic representation of the Glide Test Method-3 Inch Sample and 4 Inch Sample equipment and set-up.

DETAILED DESCRIPTION OF THE INVENTION

The Present Invention includes a polysaccharide nonwoven fibrous structure surface material formed from polysaccharide fibrous elements that is randomly bonded to a web material surface, without the use of an additional bonding step, such as thermal bonding; producing a securely bonded spun polysaccharide fibrous element surface layer using a random, non-discrete bonding process that preserves the surface layer mobility and improves softness while keeping the polysaccharide layer sufficiently anchored to the web material.

In embodiments a layer of polysaccharide, polyvinyl alcohol (PVOH), or both fiber elements is melt blown onto a web material using 1) high forming air flow and 2) a % moisture (via reduced temperature) above the Tg of the PVOH fiber elements. The inherent adhesive properties of the polysaccharide or PVOH fiber elements are used to effectively staple down and attach the elements onto the web material. The resulting layered substrate has a structure with new degrees of fiber mobility and new combinations of softness and low lint.

Typically, formulators try to form a very dry layer of polysaccharide or PVOH filaments onto a wet laid substrate by using high temperature drying air (230 °C (450 °F))) and high drying air flow rates (954 m3/hr (594 SCFM)) during the polysaccharide or PVOH spinning process. The resulting dry filaments are loose and have little fiber-to-fiber bond sites which translates to fiber mobility and surface softness. However, the loose layer of polysaccharide or PVOH filaments is not secured to the wet laid substrate and must be attached using a thermal bonding process. Thermal bonding is known to decrease surface softness and flexibility, and thermal bond spacing has been optimized to try and to balance surface softness and low lint (U.S. Pat. No. 10,814,517).

Alternatively, polysaccharide, PVOH, or both fiber elements, such as filaments can be attached to a web material by spinning the filaments onto a web material in an environment that makes the polysaccharide or PVOH slightly sticky. This is accomplished by not fully drying the filaments via reduced drying air temperature from about 150 °C to 228 °C, from about 170 °C to 224 °C, from about 190 °C to 220 °C, from about 195 °C to 210 °C and/or drying air flowrate, from about 200 m3/hr to about 720 m3/hr, from about 400 m3/hr to about 680 m3/hr, from about 540 m3/hr to about 630 m3/hr, and pulling the process air through the spun fiber layer/web material composite using high forming air vacuum from about 470 m3/hr to 1500 m3/hr, from about 580 m3/hr to 1300 m3/hr, from about 700 m3/hr to 1200 m3/hr, from about 900 m3/hr to 1050 m3/hr. Unexpectedly, when polysaccharide or PVOH filaments are formed in this manner they stay attached to the web material without requiring a thermal bonding process and furthermore the surface softness is improved compared to a polysaccharide or PVOH layer that is formed under dry conditions and is thermal bonded into web material. The reason for the improved surface feel is that the non-thermal bonded surface has a looser layer of polysaccharide or PVOH filaments, as shown in FIGS. 1A and 1B, which compare the cross-sectional SEM views of a thermal bonded FIG. 1A and a non-thermal bonded sample FIG. 1B.

DEFINITIONS

“Fibrous element” as used herein means an elongate particulate having a length greatly exceeding its average diameter, i.e. a length to average diameter ratio of at least about 10. A fibrous element may be a filament or a fiber. In embodiments, the fibrous element is a single fibrous element rather than a yarn comprising a plurality of fibrous elements.

The fibrous elements of the present invention may be spun from polymer melt compositions via suitable spinning operations, such as meltblowing and/or spunbonding and/or they may be obtained from natural sources such as vegetative sources, for example trees.

The fibrous elements of the present invention may be monocomponent and/or multicomponent.

For example, the fibrous elements may comprise bicomponent fibers and/or filaments. The bicomponent fibers and/or filaments may be in any form, such as side-by-side, core and sheath, islands-in-the-sea and the like.

“Filament” as used herein means an elongate particulate as described above that exhibits a length of greater than or equal to 5.08 cm (2 in.) and/or greater than or equal to 7.62 cm (3 in.) and/or greater than or equal to 10.16 cm (4 in.) and/or greater than or equal to 15.24 cm (6 in.).

Filaments are typically considered continuous or substantially continuous in nature. Filaments are relatively longer than fibers. Non-limiting examples of filaments include meltblown and/or spunbond filaments. Non-limiting examples of polymers that can be spun into filaments include natural polymers, such as starch, starch derivatives, cellulose, such as rayon and/or lyocell, and cellulose derivatives, hemicellulose, hemicellulose derivatives, and synthetic polymers including, but not limited to polyvinyl alcohol filaments and/or polyvinyl alcohol derivative filaments, and thermoplastic polymer filaments, such as polyesters, nylons, polyolefins such as polypropylene filaments, polyethylene filaments, and biodegradable or compostable thermoplastic fibers such as polylactic acid filaments, polyhydroxyalkanoate filaments, polyesteramide filaments, and polycaprolactone filaments. The filaments may be monocomponent or multicomponent, such as bicomponent filaments.

“Fiber” as used herein means an elongate particulate as described above that exhibits a length of less than 5.08 cm (2 in.) and/or less than 3.81 cm (1.5 in.) and/or less than 2.54 cm (1 in.). Fibers are typically considered discontinuous in nature. Non-limiting examples of fibers include pulp fibers, such as wood pulp fibers, and synthetic staple fibers such as polypropylene, polyethylene, polyester, copolymers thereof, rayon, lyocell, glass fibers and polyvinyl alcohol fibers.

Staple fibers may be produced by spinning a filament tow and then cutting the tow into segments of less than 5.08 cm (2 in.) and/or less than 3.81 cm (1.5 in.) and/or less than 2.54 cm (1 in.) thus producing fibers; namely, staple fibers.

In embodiments of the present invention, a fiber may be a naturally occurring fiber, which means it is obtained from a naturally occurring source, such as a vegetative source, for example a tree and/or plant, such as trichomes. Such fibers are typically used in papermaking and are oftentimes referred to as papermaking fibers. Papermaking fibers useful in the present invention include cellulosic fibers commonly known as wood pulp fibers. Applicable wood pulps include chemical pulps, such as Kraft, sulfite, and sulfate pulps, as well as mechanical pulps including, for example, groundwood, thermomechanical pulp and chemically modified thermomechanical pulp. Chemical pulps, however, may be preferred since they impart a superior tactile sense of softness to fibrous structures made therefrom. Pulps derived from both deciduous trees (hereinafter, also referred to as “hardwood”) and coniferous trees (hereinafter, also referred to as “softwood”) may be utilized. The hardwood and softwood fibers can be blended, or alternatively, can be deposited in layers to provide a stratified web. Also applicable to the present invention are fibers derived from recycled paper, which may contain any or all of the above categories of fibers as well as other non-fibrous polymers such as fillers, softening agents, wet and dry strength agents, and adhesives used to facilitate the original papermaking.

In embodiments, the wood pulp fibers are selected from the group consisting of hardwood pulp fibers, softwood pulp fibers, and mixtures thereof. The hardwood pulp fibers may be selected from the group consisting of: tropical hardwood pulp fibers, northern hardwood pulp fibers, and mixtures thereof. The tropical hardwood pulp fibers may be selected from the group consisting of: eucalyptus fibers, acacia fibers, and mixtures thereof. The northern hardwood pulp fibers may be selected from the group consisting of: cedar fibers, maple fibers, and mixtures thereof.

In addition to the various wood pulp fibers, other cellulosic fibers such as cotton linters, rayon, lyocell, trichomes, seed hairs, and bagasse fibers can be used in this invention. Other sources of cellulose in the form of fibers or capable of being spun into fibers include grasses and grain sources.

“Trichome” or “trichome fiber” as used herein means an epidermal attachment of a varying shape, structure and/or function of a non-seed portion of a plant. In embodiments, a trichome is an outgrowth of the epidermis of a non-seed portion of a plant. The outgrowth may extend from an epidermal cell. In one embodiment, the outgrowth is a trichome fiber. The outgrowth may be a hairlike or bristlelike outgrowth from the epidermis of a plant.

Trichome fibers are different from seed hair fibers in that they are not attached to seed portions of a plant. For example, trichome fibers, unlike seed hair fibers, are not attached to a seed or a seed pod epidermis. Cotton, kapok, milkweed, and coconut coir are non-limiting examples of seed hair fibers.

Further, trichome fibers are different from nonwood bast and/or core fibers in that they are not attached to the bast, also known as phloem, or the core, also known as xylem portions of a nonwood dicotyledonous plant stem. Non-limiting examples of plants which have been used to yield nonwood bast fibers and/or nonwood core fibers include kenaf, jute, flax, ramie and hemp.

Further trichome fibers are different from monocotyledonous plant derived fibers such as those derived from cereal straws (wheat, rye, barley, oat, etc), stalks (corn, cotton, sorghum, Hesperaloe funifera, etc.), canes (bamboo, bagasse, etc.), grasses (esparto, lemon, sabai, switchgrass, etc), since such monocotyledonous plant derived fibers are not attached to an epidermis of a plant.

Further, trichome fibers are different from leaf fibers in that they do not originate from within the leaf structure. Sisal and abaca are sometimes liberated as leaf fibers.

Finally, trichome fibers are different from wood pulp fibers since wood pulp fibers are not outgrowths from the epidermis of a plant; namely, a tree. Wood pulp fibers rather originate from the secondary xylem portion of the tree stem.

As used herein, the term “biodegradable” or “biodegradable polymer” generally refers to a material that degrades from the action of naturally occurring microorganisms, such as bacteria, fungi, and algae; environmental heat; moisture; or other environmental factors. The biodegradability of a material may be determined using ASTM Test Method 5338.92. OECD 301B is the biodegradation test used for determining compatibility of a material with wastewater treatment facilities.

As used herein “Non-discrete fiber bonding process” refers to a process in which fibrous elements (fibers or filaments) are bonded by merging, fusing, or coalescing fiber material into a substantially continuous phase such that individual fibrous elements remain as separate elements within the bonded region.

As used herein “Discrete Bonding Process” refers to a process by which individual fibrous elements are joined to one another at localized contact points to form discrete coherent bonding regions at the contact point. A discrete bonding process may include, for example: Mechanical entanglement of fibrous elements (e.g., needle punching or hydroentanglement), where fibrous elements are physically interlocked while remaining discrete; Thermal point bonding, in which discrete fibrous elements are locally softened or fused at contact points; Chemical or adhesive bonding, in which a binder material joins adjacent discrete fibrous elements.

As used herein “Wet Tack” is measured using the “Probe Tack” Test Method. This method quantifies the moist adhesive energy (mg*cm/cm2) required to separate two sheets after being pressed together in a moist, foggy localized environment, under prescribed conditions detailed here. A higher Probe Tack measurement predicts a sticky wet experience with the tissue.

“Ply” or “Plies” as used herein means an individual structure comprising one or more webs, optionally to be disposed in a substantially contiguous, face-to-face relationship with other plies, forming a multiple ply fibrous structure. It is also contemplated that a single structure can effectively form two “plies” or multiple “plies”, for example, by being folded on itself.

“Fibrous Structure” as used herein means a soft, relatively low density structure useful as a wiping implement for post-urinary and post-bowel movement cleaning (toilet tissue), for otorhinolaryngological discharges (facial tissue), multi-functional absorbent and cleaning uses (absorbent towels) and wipes, such as wet and dry wipes. The fibrous structure may be convolutedly wound upon itself about a core or without a core to form a sanitary tissue product roll or may be in the form of discrete sheets.

“Web” or “Web Material” as used herein means a structure that comprises a first web material comprising a plurality of fibrous elements, for example a plurality of fibers, such as a plurality of pulp fibers. In embodiments, the first web may comprise a plurality of wood pulp fibers. In another example, the first web material may comprise a plurality of non-wood pulp fibers, for example plant fibers, synthetic staple fibers, and mixtures thereof. In still another example, in addition to fibers, such as pulp fibers, the first web material may comprise a plurality of filaments, such as polymeric filaments, for example thermoplastic filaments such as polyolefin filaments (i.e., polypropylene filaments), thermoplastic polyvinyl alcohol filaments, and/or hydroxyl polymer filaments, for example polyvinyl alcohol filaments and/or polysaccharide filaments such as starch filaments, such as in the form of a coform web material where the fibers and filaments are commingled together and/or are present as discrete or substantially discrete layers within the first web material. In embodiments, a web material, for example a first web material, according to the present invention means an orderly arrangement of fibers and/or with filaments within a structure in order to perform a function. In embodiments, a fibrous structure according to the present invention means an association of fibrous elements that together form a structure capable of performing a function. In another example of the present invention, a fibrous structure comprises a plurality of inter-entangled fibrous elements, for example inter-entangled filaments. Non-limiting examples of web materials of the present invention include paper.

Non-limiting examples of processes for making a web material, for example a first web material, of the fibrous structures of the present invention include known wet-laid papermaking processes, for example conventional wet-pressed (CWP) papermaking processes and through-air-dried (TAD), both creped TAD and uncreped TAD, papermaking processes, and air-laid papermaking processes. Such processes typically include steps of preparing a fiber composition in the form of a fiber suspension in a medium, either wet, more specifically aqueous medium, or dry, more specifically gaseous, i.e. with air as medium. The aqueous medium used for wet-laid processes is oftentimes referred to as a fiber slurry. The fiber slurry is then used to deposit a plurality of the fibers onto a forming wire, fabric, or belt such that an embryonic web material is formed, after which drying and/or bonding the fibers together results in a web material, for example the first web material. Further processing of the first web material may be carried out such that a finished first web material is formed. For example, in typical papermaking processes, the finished first web material is the web material that is wound on the reel at the end of papermaking, often referred to as a parent roll, and may subsequently be converted into a finished fibrous structure of the present invention, e.g. a single- or multi-ply fibrous structure.

In another example, the web material, for example the first web material is a coformed web material comprising a plurality of filaments and a plurality of fibers commingled together as a result of a coforming process.

The fibrous structures of the present invention may be homogeneous or may have multiple layers. A layer is a component of a web material that may be created by supplying different fiber streams to different chambers of a stratified headbox and depositing those streams to form a layered web material. U.S. Pat. Nos. 4,300,981 and 3,994,771 disclose different methods of forming layered paper webs. For example, in wet laid structures, a stratified headbox may be supplied with a fiber stream comprising eucalyptus fibers fed a first compartment of the headbox while a different fiber stream comprising a mix of fiber types is fed to a second compartment of the headbox. The first compartment supplies fiber to the surface of the web material that will be the consumer-facing surface—the surface of the sheet that the consumer will touch when using the product. Layering eucalyptus fibers to the consumer-facing surface can provide softness benefits. In this example the layer is the portion of the web material formed from one compartment of a stratified headbox and the wet laid structure is the web material. Then a second web material, such as a web comprising spun filaments, can be combined with the first web material to create a ply. If layered, the web material may comprise at least two and/or at least three and/or at least four and/or at least five layers of fiber and/or filament compositions

In embodiments, the fibrous structure of the present invention comprises fibers, for example pulp fibers, such as cellulosic pulp fibers and more particularly wood pulp fibers.

In another example, the fibrous structure of the present invention comprises fibers and is void of filaments.

In still another example, the fibrous structures of the present invention comprises filaments and fibers, such as a co-formed fibrous structure.

“Co-formed fibrous structure” as used herein means that the fibrous structure comprises a mixture of at least two different materials wherein at least one of the materials comprises a filament, such as a polypropylene filament, and at least one other material, different from the first material, comprises a solid additive, such as a fiber and/or a particulate. In embodiments, a co-formed fibrous structure comprises solid additives, such as fibers, such as wood pulp fibers, and filaments, such as polypropylene filaments.

“Basis Weight” as used herein is the weight per unit area of a sample reported in lbs/3000 ft2 or g/m2 (gsm) and is measured according to the Basis Weight Test Method described herein.

“Machine Direction” or “MD” as used herein means the direction parallel to the flow of the fibrous structure through a fibrous structure making machine. Typically, the MD is substantially perpendicular to any perforations present in the fibrous structure.

“Cross Machine Direction” or “CD” as used herein means the direction parallel to the width of the fibrous structure making machine and perpendicular to the machine direction in the same plane.

“Embossed” as used herein with respect to a web material or a fibrous structure, means that a web material or a fibrous structure, has been subjected to a process which converts a smooth surfaced web material or fibrous structure to a decorative surface by replicating a design on one or more emboss rolls, which form a nip through which the web material or fibrous structure passes. Embossed does not include creping, microcreping, printing or other processes that may also impart a texture and/or decorative pattern to a web material or a fibrous structure.

“Differential density”, as used herein, means a web material that comprises one or more regions of relatively low fiber density, which are referred to as pillow regions, and one or more regions of relatively high fiber density, which are referred to as knuckle regions.

“Densified”, as used herein means a portion of a fibrous structure that is characterized by regions of relatively high fiber density (knuckle regions).

“Non-densified”, as used herein, means a portion of a fibrous structure that exhibits a lesser density (one or more regions of relatively lower fiber density) (pillow regions) than another portion (for example a knuckle region) of the fibrous structure.

“Non-rolled” as used herein with respect to a fibrous structure of the present invention means that the fibrous structure is an individual sheet (for example not connected to adjacent sheets by perforation lines. However, two or more individual sheets may be interleaved with one another) that is not convolutedly wound about a core or itself. For example, a non-rolled product comprises a facial tissue.

“Creped” as used herein means creped off of a Yankee dryer or other similar roll and/or fabric creped and/or belt creped. Rush transfer of a fibrous structure alone does not result in a “creped” fibrous structure for purposes of the present invention.

The fibrous structures of the present invention may exhibit a basis weight between about 1 g/m2 to about 5000 g/m2 and/or from about 10 g/m2 to about 500 g/m2 and/or from about 10 g/m2 to about 300 g/m2 and/or from about 10 g/m2 to about 120 g/m2 and/or from about 15 g/m2 to about 110 g/m2 and/or from about 20 g/m2 to about 100 g/m2 and/or from about 30 to 90 g/m2 as determined by the Basis Weight Test Method described herein. In addition, the fibrous structure of the present invention may exhibit a basis weight between about 40 g/m2 to about 120 g/m2 and/or from about 50 g/m2 to about 110 g/m2 and/or from about 55 g/m2 to about 105 g/m2 and/or from about 60 g/m2 to 100 g/m2 as determined by the Basis Weight Test Method described herein.

The fibrous structures of the present invention may exhibit a total dry tensile strength of greater than about 59 g/cm and/or from about 78 g/cm to about 394 g/cm and/or from about 98 g/cm to about 335 g/cm. In addition, the fibrous structure of the present invention may exhibit a total dry tensile strength of greater than about 196 g/cm and/or from about 196 g/cm to about 394 g/cm and/or from about 216 g/cm to about 335 g/cm and/or from about 236 g/cm to about 315 g/cm. In embodiments, the fibrous structure exhibits a total dry tensile strength of less than about 394 g/cm and/or less than about 335 g/cm.

The fibrous structures of the present invention may exhibit a density of less than 0.60 g/cm3 and/or less than 0.30 g/cm3 and/or less than 0.20 g/cm3 and/or less than 0.15 g/cm3 and/or less than 0.10 g/cm3 and/or less than 0.07 g/cm3 and/or less than 0.05 g/cm3 and/or from about 0.01 g/cm3 to about 0.20 g/cm3 and/or from about 0.02 g/cm3 to about 0.15 g/cm3 and/or from about 0.02 g/cm3 to about 0.10 g/cm3.

The fibrous structures of the present invention may be in the form of fibrous structure rolls. Such fibrous structure rolls may comprise a plurality of connected, but perforated sheets of fibrous structure, that are separably dispensable from adjacent sheets.

The fibrous structures of the present invention may comprise additives such as softening agents, temporary wet strength agents, permanent wet strength agents, bulk softening agents, lotions, silicones, wetting agents, latexes, patterned latexes and other types of additives suitable for inclusion in and/or on fibrous structures.

“Hydroxyl polymer” as used herein includes any hydroxyl-containing polymer that can be incorporated into a filament of the present invention. In embodiments, the hydroxyl polymer of the present invention includes greater than 10% and/or greater than 20% and/or greater than 25% by weight hydroxyl moieties. In another example, the hydroxyl within the hydroxyl-containing polymer is not part of a larger functional group such as a carboxylic acid group.

“Non-thermoplastic” as used herein means, with respect to a material, such as a fibrous element as a whole and/or a polymer, such as a crosslinked polymer, within a fibrous element, that the fibrous element and/or polymer exhibits no melting point and/or softening point, which allows it to flow under pressure, in the absence of a plasticizer, such as water, glycerin, sorbitol, urea and the like.

“Non-cellulose-containing” as used herein means that less than 5% and/or less than 3% and/or less than 1% and/or less than 0.1% and/or 0% by weight of cellulose polymer, cellulose derivative polymer and/or cellulose copolymer is present in fibrous element. In embodiments, “non-cellulose-containing” means that less than 5% and/or less than 3% and/or less than 1% and/or less than 0.1% and/or 0% by weight of cellulose polymer is present in fibrous element.

“Fast wetting surfactant” and/or “fast wetting surfactant component” and/or “fast wetting surfactant function” as used herein means a surfactant and/or surfactant component, such as an ion from a fast wetting surfactant, for example a sulfosuccinate diester ion (anion), that exhibits a Critical Micelle Concentration (CMC) of greater 0.15% by weight and/or at least 0.25% and/or at least 0.50% and/or at least 0.75% and/or at least 1.0% and/or at least 1.25% and/or at least 1.4% and/or less than 10.0% and/or less than 7.0% and/or less than 4.0% and/or less than 3.0% and/or less than 2.0% by weight. U.S. Pat. No. 10,696,821 to Heinzman et al., issued Jun. 30, 2020 (“the '821 patent”), describes the addition of fast-wetting surfactants to aqueous polymer melt compositions to effectively remove water from the fibrous elements during formation. When subjected to a discrete bonding process, such as thermal bonding, the resulting fibrous elements with a fast-wetting surfactant had improved mechanical properties, such as improved fail stretch, total dry stretch, and total energy absorbed (TEA).

Surprisingly, the addition of fast-wetting surfactants to fibrous structures that are not discretely bonded results in poor product performance. Particularly, when fibrous elements are formed in a high RH environment via lower drying air temperature and higher forming vacuum flow that are typically suitable for creating randomly bonded structures with low pilling and good surface feel. If the fibrous elements are formed with a fast-wetting surfactant in the composition, the resulting layered structures have high Total Pilling Volume.

“Polymer melt composition” or “Polysaccharide melt composition” as used herein means a composition comprising water and a melt processed polymer, such as a melt processed fibrous element-forming polymer, for example a melt processed hydroxyl polymer, such as a melt processed polysaccharide.

“Melt processed fibrous element-forming polymer” as used herein means any polymer, which by influence of elevated temperatures, pressure and/or external plasticizers may be softened to such a degree that it can be brought into a flowable state, and in this condition may be shaped as desired.

“Melt processed hydroxyl polymer” as used herein means any polymer that contains greater than 10% and/or greater than 20% and/or greater than 25% by weight hydroxyl groups and that has been melt processed, with or without the aid of an external plasticizer. More generally, melt processed hydroxyl polymers include polymers, which by the influence of elevated temperatures, pressure and/or external plasticizers may be softened to such a degree that they can be brought into a flowable state, and in this condition may be shaped as desired.

“Blend” as used herein means that two or more materials, such as a fibrous element-forming polymer, for example a hydroxyl polymer and a polyacrylamide are in contact with each other, such as mixed together homogeneously or non-homogeneously, within a filament. In other words, a filament formed from one material, but having an exterior coating of another material is not a blend of materials for purposes of the present invention. However, a fibrous element formed from two different materials is a blend of materials for purposes of the present invention even if the fibrous element further comprises an exterior coating of a material.

“Associate,” “Associated,” “Association,” and/or “Associating” as used herein with respect to fibrous elements and/or with respect to a surface and/or surface material being associated with a fibrous structure and/or a first web material means combining, either in direct contact or in indirect contact, fibrous elements and/or a surface material with a first web material such that a fibrous structure is formed. In another example, the fibrous elements and/or surface material may be associated with the first web material, directly or indirectly, by being deposited onto the same first web material making belt.

“Average Diameter” as used herein, with respect to a fibrous element, is measured according to the Average Diameter Test Method described herein. In embodiments, a fibrous element of the present invention exhibits an average diameter of less than 50 μm and/or less than 25 μm and/or less than 20 μm and/or less than 15 μm and/or less than 10 μm and/or less than 6 μm and/or greater than 1 μm and/or greater than 3 μm.

“3D Pattern” with respect to a fibrous structure's surface in accordance with the present invention means herein a pattern that is present on at least one surface of the fibrous structure. The 3D pattern texturizes the surface of the fibrous structure, for example by providing the surface with protrusions and/or depressions. The 3D pattern on the surface of the fibrous structure is made by making at least one fibrous structure ply on a patterned molding member that imparts the 3D pattern to the fibrous structure plies made thereon. For example, the 3D pattern may comprise a series of line elements, such as a series of line elements that are substantially oriented in the cross-machine direction of the fibrous structure.

In embodiments, a series of line elements may be arranged in a 3D pattern selected from the group consisting of: periodic patterns, aperiodic patterns, straight line patterns, curved line patterns, wavy line patterns, snaking patterns, square line patterns, triangular line patterns, S-wave patterns, sinusoidal line patterns, and mixtures thereof. In another example, a series of line elements may be arranged in a regular periodic pattern or an irregular periodic pattern (aperiodic) or a non-periodic pattern.

“Wet textured” as used herein means that a 3D patterned fibrous structure ply comprises texture (for example a three-dimensional topography) imparted to the fibrous structure and/or fibrous structure's surface during a fibrous structure making process. In embodiments, in a wet-laid fibrous structure making process, wet texture can be imparted to a fibrous structure upon fibers and/or filaments being collected on a collection device that has a three-dimensional (3D) surface which imparts a 3D surface to the fibrous structure being formed thereon and/or being transferred to a fabric and/or belt, such as a through-air-drying fabric and/or a patterned drying belt, comprising a 3D surface that imparts a 3D surface to a fibrous structure being formed thereon. In embodiments, the collection device with a 3D surface comprises a patterned, such as a patterned formed by a polymer or resin being deposited onto a base substrate, such as a fabric, in a patterned configuration. The wet texture imparted to a wet-laid fibrous structure is formed in the fibrous structure prior to and/or during drying of the fibrous structure. Non-limiting examples of collection devices and/or fabric and/or belts suitable for imparting wet texture to a fibrous structure include those fabrics and/or belts used in fabric creping and/or belt creping processes, for example as disclosed in U.S. Pat. Nos. 7,820,008 and 7,789,995, coarse through-air-drying fabrics as used in uncreped through-air-drying processes, and photo-curable resin patterned through-air-drying belts, for example as disclosed in U.S. Pat. No. 4,637,859. For purposes of the present invention, the collection devices used for imparting wet texture to the fibrous structures would be patterned to result in the fibrous structures comprising a surface pattern comprising a plurality of parallel line elements wherein at least one, two, three, or more, for example all of the parallel line elements exhibit a non-constant width along the length of the parallel line elements. This is different from non-wet texture that is imparted to a fibrous structure after the fibrous structure has been dried, for example after the water level of the fibrous structure is less than 15% and/or less than 10% and/or less than 5%. An example of non-wet texture includes embossments imparted to a fibrous structure by embossing rolls during converting of the fibrous structure.

As used herein, the term “geometric mean tensile” (GMT) refers to the square root of the product of the machine direction tensile and the cross-machine direction tensile of the web, which are determined as described in the Test Method section.

As used herein, the term “caliper” is the representative thickness of a single sheet (caliper of fibrous structures comprising two or more plies is the thickness of a single sheet of fibrous structure comprising all plies) measured in accordance with TAPPI test method T402 using an EMVECO 200-A Microgage automated micrometer (EMVECO, Inc., Newberg, Oreg.). The micrometer has an anvil diameter of 2.22 inches (56.4 mm) and an anvil pressure of 132 grams per square inch (per 6.45 square centimeters) (2.0 kPa).

As used herein, the term “slope” refers to slope of the line resulting from plotting tensile versus stretch and is an output of the MTS TestWorks™ while determining the tensile strength as described in the Test Methods section herein. Slope is reported in the units of grams (g) per unit of sample width (inches) and is measured as the gradient of the least-squares line fitted to the load-corrected strain points falling between a specimen-generated force of 70 to 157 grams (0.687 to 1.540 N) divided by the specimen width. Slopes are generally reported herein as having units of grams per 3 inch sample width or g/3″.

As used herein, the term “geometric mean slope” (GM Slope) generally refers to the square root of the product of machine direction slope and cross-machine direction slope.

As used herein, the term “stretch” generally refers to the ratio of the slack-corrected elongation of a specimen at the point it generates its peak load divided by the slack-corrected gauge length in any given orientation. Stretch is an output of the MTS TestWorks™ while determining the tensile strength as described in the Test Methods section herein. Stretch is reported as a percentage and may be reported for machine direction stretch (MDS), cross-machine direction stretch (CDS) or as geometric mean stretch (GMS), which is the square root of the product of machine direction stretch and cross-machine direction stretch.

As used herein, the term “Roll Firmness,” generally refers to the ability of a rolled fibrous structure to withstand deflection when impacted, which is determined as described in the Test Methods section.

As used herein, the term “Roll Structure” generally refers to the overall appearance and quality of a rolled fibrous structure and is the product of Roll Bulk (expressed in cc/g) and caliper (express in cm) divided by Firmness (expressed in cm). Roll Structure is generally referred to herein without reference to units.

As used herein, the term “Stiffness Index” refers to the quotient of the geometric mean slope (having units of g/3″) divided by the geometric mean tensile strength (having units of g/3″).

As used herein, the term “Surface Smoothness” refers to the filtered surface image topography measured as described in the Surface Topography Test Method section. Surface Smoothness is expressed as three different values—Sa, Sq and S90—and may have units of millimeters (mm) or microns (μm). Because of the relationship between surface topography and perceived smoothness or roughness, the relative feel of a fibrous structure may be predicted based upon its surface topography. Surface topography may be measured using profilometry, for example by the Surface Topography Test Method set forth below. Accordingly, in certain embodiments, fibrous structures of the Present Invention have improved smoothness, such as low Sa, Sq and/or S90 values. In embodiments the fibrous structures may have an Sa of from about 15 μm to about 60 μm, about 20 μm to about 50 μm, or about 25 μm to about 45 μm, as determined using the Surface Topography Test Method described herein. In embodiments the fibrous structures may have an Sq of from about 10 μm to about 80 μm, about 20 μm to about 70 μm, or about 30 μm to about 60 μm, as determined using the Surface Topography Test Method described herein.

As used herein, the term “Pilling” refers to a surface phenomenon in fibrous structures in which individual fibers or fiber segments migrate from the interior of the structure to the surface and, under mechanical abrasion or friction, entangle to form small, localized fiber agglomerates that remain at least partially attached to the fibrous structure.

As used herein, the term “Total Pilling Volume” refers to a total pilling volume that is the sum of individual equivalent pilling volumes that are binned by size and counted as reported in the Pilling Test Method.

As used herein, the term Dual Surface Peak Load or Peak Load refers to the stress required to move a strip of tissue web across the surface of a second strip of tissue webs as described in the Glide Test Method.

Unless otherwise noted, all component or composition levels are in reference to the active level of that component or composition, and are exclusive of impurities, for example, residual solvents or by-products, which may be present in commercially available sources.

As used herein, the articles including “a” and “an” when used in a claim, are understood to mean one or more of what is claimed or described.

As used herein, the terms “include”, “includes” and “including” are meant to be non-limiting.

As used herein “or” also means in addition to an alternative also includes in addition to, such as “and/or.”

All percentages and ratios are calculated by weight unless otherwise indicated. All percentages and ratios are calculated based on the total composition unless otherwise indicated.

It should be understood that every maximum numerical limitation given throughout this specification includes every lower numerical limitation, as if such lower numerical limitations were expressly written herein. Every minimum numerical limitation given throughout this specification will include every higher numerical limitation, as if such higher numerical limitations were expressly written herein. Every numerical range given throughout this specification will include every narrower numerical range that falls within such broader numerical range, as if such narrower numerical ranges were all expressly written herein.

As used herein, the word “or” when used as a connector of two or more elements is meant to include the elements individually and in combination; for example X or Y, means X or Y or both.

By “μm” or “microns” as used herein is meant micrometer.

All measurements referred to herein are made at about 23 °C (i.e. room temperature) unless otherwise specified.

Fibrous Structures

In embodiments of the present invention as shown in FIGS. 2 and 3, a fibrous structure 10 of the present invention comprises a first web material 12 comprising a plurality of fibrous elements, for example fibers 14, and a surface material 16, for example a second web material 18 comprising a plurality of fibrous elements, for example spun fibrous elements and/or non-naturally occurring fibrous elements, such as filaments 20, for example hydroxyl polymer filaments, such that the fibrous structure exhibits improved surface smoothness, low lint, good wet feel and low wet tack, for example known fibrous structures, such as known toilet tissue products and/or known skin-wiping fibrous structure products.

In embodiments, the surface material 16 comprises a plurality of fibers and/or filaments that are deposited onto the first web material 12 in a layered configuration. The surface material 16 may be in the form of a second web material 18 after being deposited onto the first web material 12.

In embodiments, as shown in FIG. 3, a surface 22 of the surface material 16 may be a consumer-contacting surface, such that during use of the fibrous structure 10 the consumer wipes the surface 22 of the surface material 16, such as the second web material 18, across the skin of the consumer or another person. The fibrous structure 10 may have a bottom surface 19 opposing the consumer contacting surface of the surface material 16. One of the benefits of the fibrous structure 10 is that it exhibits improved fiber mobility, softness, and low lint.

In embodiments, the surface material 16, for example second web material 18, may be associated with the first web material 12 by random bonding sites, producing a structure with uniform, non-patterned sites that creates a smooth surface by adhering a layer of spun filaments to a wet laid cellulosic substrate.

As shown in FIG. 4, in embodiments a multi-ply fibrous structure 26 may comprise a first fibrous structure ply 28 and a second fibrous structure ply 30 wherein at least one of the first and second fibrous structure plies 28, 30 is a fibrous structure 10 according to the present invention. In this case, both the first and second fibrous structure plies 28, 30 are fibrous structures 10 according to the present invention. The first and second fibrous structure plies 28, 30 may be associated with one another by bonding, such as thermal bond sites and/or adding an adhesive to form adhesive bond sites 32 as shown. The first and second fibrous structure plies 28, 30 are associated with one another such that the surface material 16 of both the first and second fibrous structure plies 28, 30 form exterior surfaces of the multi-ply fibrous structure 26 and the first web material 12 of both the first and second fibrous structure plies 28, 30 form inner web materials within the multi-ply fibrous structure 26.

In embodiments, a multi-ply fibrous structure 26 according to the present invention may comprise a first fibrous structure ply 28 and a second fibrous structure ply 30, which may be glued together by adhesive bond sites 32 to form the multi-ply fibrous structure 26. The first fibrous structure ply 28 comprises an exterior layer, the surface material 16, for example the second web material 18, comprising a plurality of fibrous elements, for example a plurality of filaments 20, such as polysaccharide or hydroxyl polymer filaments, for example PVOH filaments, and an additional layer, the first web material 12, which comprises a plurality of fibrous elements, for example a plurality of fibers, such as pulp fibers, for example wood pulp fibers, present at a level of greater than about 0.30 gsm to about 3.0 gsm, greater than 6 gsm and/or greater than 8 gsm and/or greater than greater than 10 gsm and/or greater than 12 gsm and/or greater than 14 gsm and/or greater than 16 gsm and/or at least 18 gsm and/or less than 55 gsm and/or less than 50 gsm and/or less than 40 gsm and/or less than 35 gsm.

As shown in FIG. 5, in another example of the present invention, the fibrous structure 10 comprises one or more voids 34 (vacuoles) defined by two different materials, for example both the surface material 16 and the first web material 12. A void 34 may be formed by the surface material 16 bridging a texture, such as a depression or channel, such as imparted to a surface of the first web material 12 by a patterned molding member, for example a patterned resin molding member and/or a through-air-drying fabric, such as a coarse through-air-drying fabric, for example as is used in the UCTAD process, and/or an embossing operation and/or a creping operation, such as a belt creping operation and/or a fabric creping operation and/or creping off a drying cylinder, such as a Yankee. The voids 34 of the fibrous structures 10 may be seen using different imaging tools, such as μCT.

As also shown in FIG. 5, the fibrous structure 10 of the present invention may comprise differential planar materials relative to each other, for example a monoplanar material, for example the surface material 16, and a multi-planar material, for example the first web material 12 that comprises a texture.

In embodiments, the surface material 16 may comprise a water soluble polymer, such as a semi-crystalline polymer, for example starch and/or starch derivative and/or polyvinylalcohol, and the first web material 12 may comprise a water insoluble polymer, such as a highly crystalline polymer, for example cellulose.

In another example, the surface material 16, for example the second web material 18 may comprise a plurality of fibrous elements, for example a plurality of smooth fibrous elements, such as smooth spun filaments, in other words, the exterior surface of the fibrous elements is non-textured, at least relative to the fibrous elements of the first web material 12, for example pulp fibers, such as wood pulp fibers, which are textured (rough) relative to the smooth fibrous elements of the second web material 18.

In still another example, the surface material 16, for example the second web material 18 may comprise a plurality of fibrous elements, for example filaments 20, that exhibit an average diameter (less than 10 μm) less than the average diameter (greater than 10 μm and/or greater than 12 μm) of the fibrous elements, for example fibers 14, such as pulp fibers, of the first web material 12.

In still yet another example, the surface material 16, for example the second web material 18 may comprise a plurality of fibrous elements, for example filaments 20, that exhibit a length (greater than 5.08 cm) greater than the length (5.08 cm or less) of the fibrous elements, for example fibers 14, such as pulp fibers, of the first web material 12.

In embodiments, the fibrous structure 10 of the present invention may be made by the fibrous structure making process 40 shown in FIG. 6 by providing a first web material 12 comprising a plurality of fibrous elements, for example fibers 14, and depositing a surface material 16, for example a plurality of fibrous elements, for example filaments 20, from one or more surface material sources 21, such as a die, for example a meltblow die, such as a multi-row capillary die as shown in FIG. 7 in this case to form a second web material 18 of inter-entangled fibrous elements, for example filaments 20, onto at least one surface of the first web material 12 to form the fibrous structure 10 of the present invention. Wherein the fibrous elements, for example filaments 20 when deposited on the at least one surface of the first web material 12 have a water (moisture) content providing them with sufficient tackiness to adhere to the surface without the need for an additional bonding step, such as thermal boding. In embodiments the fibrous elements of the first web material may have a water content of from about 1% to about 25%, about 1% to about 20%, about 1% to about 15%, about 1% to about 10%, about 2% to about 10%, and all ranges in between, as determined using the Filament Moisture Content described herein. In embodiments the fibrous elements of the first web material may have a water content 30 seconds after contacting the first web material of from about 11% to about 25%, about 1% to about 20%, about 1% to about 15%, about 1% to about 10%, about 2% to about 10%, and all ranges in between, as determined using the Filament Moisture Content described herein. Further, a vacuum 27 may be applied to a bottom surface 19 of the fibrous structure 10, pulling humid air through the fibrous structure 10 serving to preserve the water content of the surface material 16 and increase contact between the fibrous elements of the surface material and the first web material 12. When a second surface material is applied to the fibrous structure 10, at least one of the surface material sources 21 deposits the second surface material, such that the first surface material is positioned between the first web material 12 and the second surface material. The fibrous structure making process 40 further comprises the step of bonding the surface material 16 to the first web material 12 by increasing the water content of the surface material 16, for example by less drying during the spinning process. The fibrous structure making process 40 may optionally comprise the step of winding the fibrous structure 10 into a roll, such as a parent roll for unwinding in a converting operation to cut the roll into consumer-useable sized fibrous structure rolls and/or emboss the fibrous structure and/or perforate the fibrous structure into consumer-useable sized sheets of fibrous structure. In addition, the roll of fibrous structure may be combined with another fibrous structure ply, the same or different as the roll of fibrous structure to make a multi-ply fibrous structure 26 according to the present invention, an example of which is shown in FIG. 4.

The multi-row capillary die (surface material source 21) shown in FIG. 7 comprises at least one fibrous element-forming hole 23, and/or 2 or more and/or 3 or more rows of fibrous element-forming holes 23 from which filaments are spun. At least one row of the fibrous element-forming holes 23 contains 2 or more and/or 3 or more and/or 10 or more fibrous element-forming holes 23. In addition to the fibrous element-forming holes 23, the multi-row capillary die comprises fluid-releasing holes 25, such as gas-releasing holes, in embodiments air-releasing holes, that provide attenuation to the filaments formed from the fibrous element-forming holes 23. One or more fluid-releasing holes 25 may be associated with a fibrous element-forming hole 23 such that the fluid exiting the fluid-releasing hole 25 is parallel or substantially parallel (rather than angled like a knife-edge die) to an exterior surface of a filament exiting the fibrous element-forming hole 23. In embodiments, the fluid exiting the fluid-releasing hole 25 contacts the exterior surface of a filament formed from a fibrous element-forming hole 23 at an angle of less than 30° and/or less than 20° and/or less than 10° and/or less than 5° and/or about 0°. One or more fluid releasing holes 25 may be arranged around a fibrous element-forming hole 23. In embodiments, one or more fluid-releasing holes 25 are associated with a single fibrous element-forming hole 23 such that the fluid exiting the one or more fluid releasing holes 25 contacts the exterior surface of a single filament formed from the single fibrous element-forming hole 23. In embodiments, the fluid-releasing hole 25 permits a fluid, such as a gas, for example air, to contact the exterior surface of a filament formed from a fibrous element-forming hole 23 rather than contacting an inner surface of a filament, such as what happens when a hollow filament is formed.

In embodiments, one or more plies of the fibrous structure according to the present invention may be combined, for example with glue, with another ply of fibrous structure, which may also be a fibrous structure according to the present invention, to form a multi-ply fibrous structure. In embodiments, the multi-ply fibrous structure may be formed by combining two or more plies of fibrous structure according to the present invention.

Surprisingly, it has been found that by keeping a higher water content in extruded fibrous elements, such as filaments it allows for multiple benefits in a fibrous structure. The higher water content is achieved in embodiments by reducing the amount of water removed from the fibrous elements via a higher humidity environment prior to them contacting a web material, in embodiments the humidity may be from about from about 10% RH to about 70% RH, about 20% to about 60%, or from about 20% to about 50%. This provides the fibrous elements with a sufficient tackiness to adhere to a web material surface, which when dried bonds the fibrous element surface material to the web material allowing the fibrous elements more mobility, see FIG. 1B as compared to surface material which has been thermally bonded, see FIG. 1A to the web material. The “tackiness” of the fibrous elements is determined by measuring modulus, wherein the modulus may be from about 0.1 GPa to about 30 GPa, about 0.2 GPa to about 20 GPa, about 0.3 GPa to about 10 GPa, less than 30 GPa, or less than 20 GPa. Unexpectedly the bond formed by drying is strong enough to adhere the surface material to the web material but also provides the fibrous structure with increased softness and low pilling—as compared to thermally bonded fibrous structures. In embodiments the fibrous structures may have a pilling of less than 1,500 m3, less than 1,000 m3, less than 500 m3, less than 300 m3, less than 100 m3, less than 50 m3, less than 20 m3, less than 10 m3, or from about 1 mm3 to about −1300 mm3, from about 1 mm3 to about 1100 mm3, from about 1 mm3 to about 900 mm3, from about 1 mm3 to about 750 mm3, from about 100 mm3 to about 700 mm3, or from about 100 mm3 to about 600 mm3. The strength of the dried bond between the fibrous elements of the surface material and the web material is determined by measuring ply bond, wherein the ply bond may be greater than 12 g, from about 11 g to about 25 g, or from about 15 g to about 20 g. The softness of the fibrous structure is measured by determining TS7 which in embodiments is from about 3 dB V2 rms to about 10 dB V2 rms, from about 3 dB V2 rms to about 6 dB V2 rms, from about 3.5 dB V2 rms to about 5.5 dB V2 rms, or is less than 8.5 dB V2 as measured by the Emtec Test Method.

In another example, the fibrous structures of the present invention may be creped or uncreped. In embodiments, the fibrous structures of the present invention are uncreped fibrous structures. In embodiments, the exterior surface of the fibrous structure of the present invention, for example surface 22 of the surface material 16 is not creped (uncreped and/or non-undulating and/or not creped off a surface, such as a Yankee), however the first web material 12 may be creped (undulating and/or creped off a surface, such as a Yankee).

In addition to the fibrous structures of the present invention exhibiting improved surface properties as described herein, such fibrous structures also may exhibit improved cleaning properties, for example bowel movement cleaning properties, compared to known fibrous structures, for example known fibrous structures comprising hydroxyl polymer filaments and known fibrous structures, such as wet-laid and/or air-laid, comprising cellulose fibers, for example pulp fibers. Without wishing to be bound by theory, it is believed that the fibrous structures of the present invention exhibit improved skin benefit and/or glide on skin properties and/or cleaning properties due to the hydroxyl polymer fibrous elements of the present invention exhibiting greater absorbency, without a gooey feel, than pulp fibers, and therefore facilitates better, in reality and/or perception, absorption of bowel movement and/or urine more completely and/or faster than known fibrous structures. In addition, it is believed that the fibrous structures of the present invention that comprise a plurality of hydroxyl polymer fibrous elements, for example hydroxyl polymer filaments in an exterior layer, such as a scrim, provides an improved absorbency, without a gooey feel, than known fibrous structures, such that the hydroxyl polymer fibrous elements during use contact the user's skin surface and trap and/or lock in the bowel movement or portions thereof. Further, it is believed that the fibrous structures of the present invention that comprise a plurality of hydroxyl polymer fibrous elements, for example hydroxyl polymer filaments in an exterior layer that provide improved surface properties permits a user to apply more force to the fibrous structure during use because the hydroxyl polymer fibrous elements provide a cushion and/or buffer compared to known fibrous structures, especially known wet-laid and/or air-laid fibrous structures that consist or consist essentially of pulp fibers.

The fibrous structures of the present invention may be embossed and/or tufted that creates a three-dimensional surface pattern that provides aesthetics and/or improved cleaning properties. The level of improved cleaning properties relates to the % contact area under a load, such as a user's force applied to the fibrous structure during wiping, and/or % volume/area under a load, such as a user's force applied to the fibrous structure during wiping, created by the three-dimensional surface pattern on the surface of the fibrous structure. In embodiments, the emboss area may be greater than 10% and/or greater than 12% and/or greater than 15% and/or greater than 20% of the surface area of at least one surface of the fibrous structure.

The fibrous structure of the present invention may also exhibit an CRT Initial Rate at 2 Seconds of greater than 0.50 and/or greater than 0.75 and/or greater than 1.00 and/or greater than 1.25 and/or greater than 1.50 and/or greater than 2.00 and/or greater than 2.25 and/or greater than 2.40 g/2 seconds as measured according to the CRT Test Method described herein.

The fibrous structure of the present invention may comprise two or more components, for example a first component comprising a first web material that exhibits a different bulk density from the second component, such as a the surface material. In embodiments, the first web material exhibits a lower bulk density than the surface material, for example second web material as determined according to the μCT (Micro-CT) Test Method described herein.

In one example, the layered fibrous structures of the present invention exhibit a Dual Surface Peak Load value of greater than about 5 g, greater than about 15 g, greater than about 20 g, greater than about 30 g to less than about 120 g, to less than about 100 g, or to less than about 90 g as measured according to the Glide Test Method-4 Inch Sample described herein. It has unexpectedly been found that fibrous structures, for example layered fibrous structures, that exhibit a Peak Load value of less than 10 g are considered too slippery/slick and provide poor bowel movement cleaning during use. Further, it has unexpectedly been found that fibrous structures, for example layered fibrous structures, that exhibit a Dual Surface Peak Load value of greater than 90 g result in roll dispensing negatives, for example where the consumer cannot find the tail end of the roll for easy/hassle free dispensing during use.

The fibrous structure comprises a least one surface, a consumer-contacting surface, that comes into contact with a consumer during use, such as during wiping. The surface of the fibrous structure may comprise and/or be defined by at least a portion of the first web material.

In embodiments, the fibrous structure of the present invention is a layered (as used herein “layered” in this context means the fibrous structure is not made up of separate plies of fibrous structures or web materials that are associated with one another to form a multi-ply fibrous structure, but rather is made up of a first web material upon which a surface material (not in the form of a pre-formed web material, but rather in the form of fibrous elements) is deposited, directly or indirectly, onto the first web material), and optionally dispersible (as used herein “dispersible” means aerobic biodisintegratable as measured according to EDANA FG505 Aerobic Biodisintegration Test) fibrous structure.

In embodiments, the fibrous structure is a wet fibrous structure, for example a fibrous structure comprising a liquid composition.

First Web Material

The first web material comprises a plurality of fibrous elements, for example a plurality of fibers, such as greater than 80% and/or greater than 90% and/or greater than 95% and/or greater than 98% and/or greater than 99% and/or 100% by weight of the first web material of fibers.

In embodiments, the first web material comprises a plurality of naturally-occurring fibers, for example pulp fibers, such as wood pulp fibers (hardwood and/or softwood pulp fibers). In another example, the first web material comprises a plurality of non-naturally occurring fibers (synthetic fibers), for example staple fibers, such as rayon, lyocell, polyester fibers, polycaprolactone fibers, polylactic acid fibers, polyhydroxyalkanoate fibers, and mixtures thereof. In another example, the first web material comprises a mixture of naturally-occurring fibers, for example pulp fibers, such as wood pulp fibers (hardwood and/or softwood pulp fibers) and a plurality of non-naturally occurring fibers (synthetic fibers), for example staple fibers, such as rayon, lyocell, polyester fibers, polycaprolactone fibers, polylactic acid fibers, polyhydroxyalkanoate fibers, and mixtures thereof.

The first web material may comprise one or more filaments, such as polyolefin filaments, which are not dispersible, for example polypropylene and/or polyethylene filaments, starch filaments, starch derivative filaments, cellulose filaments, polyvinyl alcohol filaments.

The first web material of the present invention may be single-ply or multi-ply web material. In other words, the first web materials of the present invention may comprise one or more first web materials, the same or different from each other so long as one of them comprises a plurality of pulp fibers.

In embodiments, the first web material comprises a wet laid fibrous structure ply, such as a through-air-dried fibrous structure ply, for example an uncreped, through-air-dried fibrous structure ply and/or a creped, through-air-dried fibrous structure ply.

In another example, the first web material and/or wet laid fibrous structure ply may exhibit substantially uniform density.

In another example, the first web material and/or wet laid fibrous structure ply may exhibit differential density.

In another example, the first web material and/or wet laid fibrous structure ply may comprise a surface pattern

In embodiments, the wet laid fibrous structure ply comprises a conventional wet-pressed fibrous structure ply. The wet laid fibrous structure ply may comprise a fabric-creped fibrous structure ply. The wet laid fibrous structure ply may comprise a belt-creped fibrous structure ply.

In still another example, the first web material may comprise an air laid fibrous structure ply.

The first web materials of the present invention may comprise a surface softening agent or be void of a surface softening agent, such as silicones, quaternary ammonium compounds, lotions, and mixtures thereof. In embodiments, the fibrous structure is a non-lotioned first web material.

The first web materials of the present invention may comprise trichome fibers or may be void of trichome fibers.

Non-Limiting Examples of Making First Web Materials

The first web materials of the present invention may be made by any suitable papermaking process, such as conventional wet press papermaking process, through-air-dried papermaking process, belt-creped papermaking process, fabric-creped papermaking process, creped papermaking process, uncreped papermaking process, coform process, and air-laid process, so long as the first web material comprises a plurality of fibers. In embodiments, the first web material is made on a molding member of the present invention is used to make the first web material of the present invention. The method may be a first web material making process that uses a cylindrical dryer such as a Yankee (a Yankee-process) or it may be a Yankeeless process as is used to make substantially uniform density and/or uncreped first web materials (fibrous structures). Alternatively, the first web materials may be made by an air-laid process and/or meltblown and/or spunbond processes and any combinations thereof so long as the first web materials of the present invention are made thereby.

As shown in FIG. 8, one example of a process and equipment, represented as 66 for making a first web material according to the present invention comprises supplying an aqueous dispersion of fibers (a fibrous furnish or fiber slurry) to a headbox 68 which can be of any convenient design. From headbox 68 the aqueous dispersion of fibers is delivered to a first foraminous member 70 which is typically a Fourdrinier wire, to produce an embryonic fibrous structure 72.

The first foraminous member 70 may be supported by a breast roll 74 and a plurality of return rolls 76 of which only two are shown. The first foraminous member 70 can be propelled in the direction indicated by directional arrow 78 by a drive means. Optional auxiliary units and/or devices commonly associated fibrous structure making machines and with the first foraminous member 70, include forming boards, hydrofoils, vacuum boxes, tension rolls, support rolls, wire cleaning showers, and the like.

After the aqueous dispersion of fibers is deposited onto the first foraminous member 70, embryonic fibrous structure 72 is formed, typically by the removal of a portion of the aqueous dispersing medium by techniques well known to those skilled in the art. Vacuum boxes, forming boards, hydrofoils, and the like are useful in effecting water removal. The embryonic web material 72 may travel with the first foraminous member 70 about return roll 76 and is brought into contact with a patterned molding member 50, such as a 3D patterned through-air-drying belt. While in contact with the patterned molding member 50, the embryonic web material 72 will be deflected, rearranged, and/or further dewatered. This can be accomplished by applying differential speeds and/or pressures.

The patterned molding member 50 may be in the form of an endless belt. In this simplified representation, the patterned molding member 50 passes around and about patterned molding member return rolls 82 and impression nip roll 84 and may travel in the direction indicated by directional arrow 86. Associated with patterned molding member 50, but not shown, may be various support rolls, other return rolls, cleaning means, drive means, and the like well known to those skilled in the art that may be commonly used in fibrous structure making machines.

After the embryonic web material 72 has been associated with the patterned molding member 50, fibers within the embryonic web material 72 are deflected into pillows (“deflection conduits”) present in the patterned molding member 50. In embodiments of this process step, there is essentially no water removal from the embryonic web material 72 through the deflection conduits after the embryonic web material 72 has been associated with the patterned molding member 50 but prior to the deflecting of the fibers into the deflection conduits. Further water removal from the embryonic web material 72 can occur during and/or after the time the fibers are being deflected into the deflection conduits. Water removal from the embryonic web material 72 may continue until the consistency of the embryonic web material 72 associated with patterned molding member 50 is increased to from about 25% to about 35%. Once this consistency of the embryonic web material 72 is achieved, then the embryonic web material 72 can be referred to as an intermediate web material 88. During the process of forming the embryonic web material 72, sufficient water may be removed, such as by a non-compressive process, from the embryonic web material 72 before it becomes associated with the patterned molding member 50 so that the consistency of the embryonic web material 72 may be from about 10% to about 30%.

As noted, water removal occurs both during and after deflection; this water removal may result in a decrease in fiber mobility in the embryonic web material. This decrease in fiber mobility may tend to fix and/or freeze the fibers in place after they have been deflected and rearranged. The drying of the web material in a later step in the process of this invention may serve to more firmly fix and/or freeze the fibers in position.

Any convenient means conventionally known in the papermaking art can be used to dry the intermediate web material 88. Examples of such suitable drying process include subjecting the intermediate web material 88 to conventional and/or flow-through dryers and/or Yankee dryers.

In embodiments of a drying process, the intermediate web material 88 in association with the patterned molding member 50 passes around one or more patterned molding member return rolls 82 and travels in the direction indicated by directional arrow 86. The intermediate web material 88 may pass through an optional predryer 90. This predryer 90 can be a conventional flow-through dryer (hot air dryer) well known to those skilled in the art. In addition, the predryer 90 can also be a so-called capillary dewatering apparatus. In such an apparatus, the intermediate web material 88 passes over a sector of a cylinder having preferential-capillary-size pores through its cylindrical-shaped porous cover. Further, the predryer 90 can be a combination capillary dewatering apparatus and flow-through dryer. The quantity of water removed in the predryer 90 may be controlled so that a predried web material 92 exiting the predryer 90 has a consistency (percent solids in the sheet—a measure of dryness) of from about 30% to about 98%. The predried web material 92, which may still be associated with patterned molding member 50, may pass around another patterned molding member return roll 82 and as it travels to an impression nip roll 84. As the predried web material 92 passes through the nip formed between impression nip roll 84 and a surface of a Yankee dryer 94, the pattern formed by the top surface 96 of patterned molding member 50 is impressed into the predried web material 92 to form a 3D patterned web material 98, a first web material of the present invention. The 3D patterned web material 98 can then be adhered to the surface of the Yankee dryer 94 where it can be dried to a consistency of at least about 95%.

The 3D patterned web material 98 can then be foreshortened by creping (creped off the Yankee) the 3D patterned web material 98 with a creping blade 97 to remove the 3D patterned web material 98 from the surface of the Yankee dryer 94 resulting in the production of a 3D patterned creped web material 99, which is a non-limiting example of a first web material in accordance with the present invention. As used herein, foreshortening refers to the reduction in length, in the machine direction, of a dry (having a consistency of at least about 90% and/or at least about 95%) web material which occurs when energy is applied to the dry web material in such a way that the length of the dry web material is reduced and the fibers in the dry web material are rearranged with an accompanying disruption of fiber-fiber bonds. Foreshortening can be accomplished in any of several well-known ways. One common method of foreshortening is creping. Further, the 3D patterned creped web material 99 may be subjected to post processing steps such as calendaring, tuft generating operations, and/or embossing and/or converting.

Surface Material

In addition to the first web material, the fibrous structure of the present invention includes a surface material comprising polysaccharide or PVOH fibrous elements. The surface material of the fibrous structure is different from the first web material. The surface material may be associated with the first web material, directly (meaning in direct contact with a surface of the first web material). In embodiments, the surface material is associated with the first web material through one or more bond sites, for example at least one of the bond sites comprise a thermal bond and/or at least one of the bond sites comprises an adhesive bond. In another example, the surface material may be indirectly bonded to a surface of the first web material by being bonded to one or more intermediate materials positioned between the surface of the first web material and the surface material. The intermediate materials may be fibrous elements, web materials, liquids, particles, and/or surface coatings, such as surface softening agents, present on the surface of the first web material.

Fibrous Elements

In embodiments the fibrous elements of the present invention include polysaccharide.

In embodiments the fibrous elements of the present invention include PVOH.

In embodiments the fibrous elements of the present invention, including higher-water content polysaccharide or PVOH fibrous elements may be produced from a blended polymer melt composition, for example a blended hydroxyl polymer melt composition such as a blended aqueous hydroxyl polymer melt composition.

In embodiments, the fibrous element of the present invention is void of thermoplastic, water-insoluble polymers.

Polysaccharide or PVOH fibrous elements may have a different degrees of hydrolysis, for instance a medium degree of hydrolysis (about 70% to about 90%) or a high degrees of hydrolysis (>90%).

In embodiments, the fibrous element-forming polymers may be present in the aqueous hydroxyl polymer melt composition at an amount of from about 20% to about 50% and/or from about 30% to about 50% and/or from about 35% to about 48% by weight of the aqueous hydroxyl polymer melt composition and present in a polymeric structure, for example fibrous element and/or fibrous structure, at a level of from about 50% to about 100% and/or from about 60% to about 98% and/or from about 75% to about 95% by weight of the polymeric structure, for example fibrous element and/or fibrous structure.

Polymer Melt Composition

The polymer melt composition, for example an aqueous polymer melt composition such as an aqueous hydroxyl polymer melt composition, of the present invention comprises a melt processed fibrous element-forming polymer, such as a melt processed hydroxyl polymer.

The polymer melt compositions may already be formed or a melt processing step may need to be performed to convert a raw material fibrous element-forming polymer, such as a hydroxyl polymer, into a melt processed fibrous element-forming polymer, such as a melt processed hydroxyl polymer, thus producing the polymer melt composition. Any suitable melt processing step known in the art may be used to convert the raw material fibrous element-forming polymer into the melt processed fibrous element-forming polymer. “Melt processing” as used herein means any operation and/or process by which a polymer is softened to such a degree that it can be brought into a flowable state.

The polymer melt compositions may have a temperature of from about 50 °C to about 100 °C and/or from about 65 °C to about 95 °C and/or from about 70 °C to about 90 °C when spinning fibrous elements from the polymer melt compositions.

In embodiments, the polymer melt composition of the present invention may comprise from about 30% and/or from about 40% and/or from about 45% and/or from about 50% to about 75% and/or to about 80% and/or to about 85% and/or to about 90% and/or to about 95% and/or to about 99.5% by weight of the polymer melt composition of a fibrous element-forming polymer, such as a hydroxyl polymer. The fibrous element-forming polymer, such as a hydroxyl polymer, may have a weight average molecular weight greater than 10,000 g/mol.

The fibrous elements of the present invention may include melt spun fibers and/or spunbond fibers, staple fibers, hollow fibers, shaped fibers, such as multi-lobal fibers and multicomponent fibers, especially bicomponent fibers. The multicomponent fibers, especially bicomponent fibers, may be in a side-by-side, sheath-core, segmented pie, ribbon, islands-in-the-sea configuration, or any combination thereof. The sheath may be continuous or non-continuous around the core. The ratio of the weight of the sheath to the core can be from about 5:95 to about 95:5. The fibers of the present invention may have different geometries that include round, elliptical, star shaped, rectangular, and other various eccentricities.

In embodiments, the fibrous structures of the present invention comprise a plurality of fibrous elements, for example hydroxyl polymer filaments comprising a hydroxyl polymer. In another example, the fibrous structures may comprise starch and/or starch derivative filaments. The starch filaments may further comprise polyvinyl alcohol and/or other polymers.

Non-Limiting Example of a Fibrous Structure

A polymer melt composition comprising 50% Poval 5-88 and 50% Poval 10-98 commercially available from Kuraray Co. Ltd., Tokyo, Japan, is mixed with water and extruded from a co-rotating twin screw extruder at approximately 60% solids. The aqueous blended PVOH melt composition reaches a peak temperature between 12° and 170 °C at the exit of the extruder, and then passes through a static mixer where the melt composition is further diluted with water to 42% solids. The melt composition is then metered to a melt blown spinneret (melt blowing die) and attenuated with 65 °C saturated air stream. The filaments are dried in the spin line using 232 °C convective drying air to form a nonwoven layer of blended PVOH filaments with a basis weight between 1.0 and 4.0 g/m2. The filaments are directly spun and deposited on a first web material (a pre-formed cellulosic web) to form a fibrous structure according to the present invention. The meltblown filaments in the fibrous structure are essentially continuous filaments.

The first web material (pre-formed cellulosic web) of the fibrous structure has a basis weight of from about 10 gsm to about 50 gsm. It is produced from a wet laid papermaking process commonly known in the art. The cellulosic web can be made creped or uncreped, patterned or unpatterned.

The fibrous structure is then subjected to a thermal bonding process wherein the thermal bond sites are formed with heat and pressure. The fibrous structure is then rewound into a single ply parent roll.

The single ply parent roll is then converted into a fibrous structure with perforations and an emboss pattern. Alternatively, two parent rolls may be used to convert into a 2 ply fibrous structure.

Test Methods

Unless otherwise specified, all tests described herein including those described under the Definitions section and the following test methods are conducted on samples that have been conditioned in a conditioned room at a temperature of 23 °C±1.0 °C and a relative humidity of 50%±2% for a minimum of 24 hours prior to the test. All plastic and paper board packaging articles of manufacture, if any, must be carefully removed from the samples prior to testing. The samples tested are “usable units.” “Usable units” as used herein means sheets, flats from roll stock, pre-converted flats, fibrous structure, and/or single or multi-ply products. Except where noted all tests are conducted in such conditioned room, all tests are conducted under the same environmental conditions and in such conditioned room. Discard any damaged product. Do not test samples that have defects such as wrinkles, tears, holes, and like. All instruments are calibrated according to manufacturer's specifications.

Modulus Versus Relative Humidity and Temperature Purpose

Measure tensile modulus versus relative humidity and temperature over the relative humidity range of 0% to 60% and temperature range of 45 °C to 75 °C.

Equipment Used

    • TA Instruments Q800 DMA S/N 0800-0617 with Tension: Film clamp (TA Instruments, New Castle, DE)
    • TA Instruments DMA Relative humidity accessory S/N DMA RH-0007
    • 25.4 mm wide JDC strip cutter (Thwing Albert Cat 1-10 S/N J294); (Thwing-Albert Instrument Company, West Berlin, NJ)
    • Hydraulic Press with 20000 lb capacity. Carver Press model 3851-0 S/N 430000-625 (Carver, Inc., Wabash, IN)
    • Analytical balance with 0.00001 gram resolution. Mettler Toledo XSE205 S/N B425713719 (Mettler-Toledo, LLC, Columbus, OH)
    • 5.3 mm wide strip cutter (provided by TA Instruments).
    • Paper cutter or scissors

Sample Prep:

    • Sample-nonwoven web with the MD direction indicated.
    • Prepare nonwoven sample for Dynamic Mechanical Analysis (DMA).
      • With paper cutter, cut four pieces of nonwoven to approximately 100 mm length in CD direction by 50 mm wide in MD direction.
      • Stack the four pieces nonwoven to produce four layers, such that all layers are aligned in the MD/CD directions.
      • Using a hydraulic press, compress the four layers together with 20,000 pounds force to press the layers together, forming a single ‘mat’ of material.
      • Using 1″ wide JDC cutter, cut the mat to 25.4 mm wide in the MD direction, While the CD direction length remains 100 mm long at this stage.
      • Using 5.3 mm wide die cutter, cut 5.3 mm wide sample in the CD direction. Resulting sample are 25.4 mm long in MD direction by 5.3 mm wide in CD direction
    • Using five place analytical balance measure and record sample mass to 0.00001 grams.
    • Calculate sample thickness with the equation


Thickness (mm)=(1000*mass)/(Length*width*density), where

      • Mass=sample mass in grams
      • Length=25.4 mm
      • Width=5.3 mm
      • Density=Density of PVOH=1.19 (Literature value)

Experiment Procedure

    • Install Tension: Film clamp in Q800 DMA.
    • Calibrate clamp mass, position, and compliance.
    • Load sample into clamp with a gage length of approximately 10 mm.
    • Test is programmed and run through TA Instruments Advantage Software, settings:
      • Module: DMA Multi-Frequency-Strain
      • Method: RH sweep/Temperature Step
      • Program
        • Step 1: Date Storage Off
        • Step 2: Relative Humidity 0.0%
        • Step 3: Equilibrate at 30 C
        • Step 4: Isothermal for 20 minutes
        • Step 5: Data Storage On
        • Step 6: Isothermal for 5 minutes
        • Step 7: Step relative humidity 0.5% for 1.0 minute to 65%
        • Step 8: Isothermal for 20 minutes
        • Step 9: Data Storage Off
        • Step 10: Relative Humidity 0.0%
        • Step 11: Increment 15 °C
        • Step 12: Isothermal for 5 min
        • Step 13: Repeat Step 4 until 90 °C
      • Amplitude=15 μm
      • Frequency=4 Hz
      • Static Force=1.0 N
      • Force Track=125%
      • Sample Rate=1 pt per 10 seconds
      • Signals Collected: Time (min), Temp (C), Storage Modulus (MPa), Stiffness (N/m), Sample Sensor RH (%).

Basis Weight Test Method

Basis weight of a fibrous structure is measured on stacks of twelve usable units using a top loading analytical balance with a resolution of +0.001 g. The balance is protected from air drafts and other disturbances using a draft shield. A precision cutting die, measuring 8.890 cm±0.00889 cm by 8.890 cm±0.00889 cm is used to prepare all samples.

With a precision cutting die, cut the samples into squares. Combine the cut squares to form a stack twelve samples thick. Measure the mass of the sample stack and record the result to the nearest 0.001 g.

The Basis Weight is calculated in g/m2 as follows:


Basis Weight=(Mass of stack)/[(Area of 1 square in stack)×(No. of squares in stack)]


Basis Weight (g/m2)=Mass of stack (g)/[79.032 (cm2)/10,000 (cm2/m2)×12]

Report result to the nearest 0.1 g/m2. Sample dimensions can be changed or varied using a similar precision cutter as mentioned above, so as at least 645 square centimeters of sample area is in the stack.

Average Diameter Test Method

This Average Diameter Test Method is used to determine the average diameters of fibrous elements, such as filaments and/or fibers, where their known average diameters are not already known. For example, average diameters of commercially available fibers, such as rayon fibers, have known lengths whereas average diameters of spun filaments, such as spun hydroxyl polymer filaments, would be determined as set forth immediately below. Further, pulp fibers, such as wood pulp fibers, especially commercially available wood pulp fibers would have known diameter (width) from the supplier of the wood pulp or are generally known in the industry and/or can ultimately be measured according to the Kajaani FiberLab Fiber Analyzer SubTest Method described below.

A fibrous structure comprising filaments of appropriate basis weight (approximately 5 to 20 grams/square meter) is cut into a rectangular shape sample, approximately 20 mm by 35 mm. The sample is then coated using a SEM sputter coater (EMS Inc, PA, USA) with gold so as to make the filaments relatively opaque. Typical coating thickness is between 50 and 250 nm. The sample is then mounted between two standard microscope slides and compressed together using small binder clips. The sample is imaged using a 10× objective on an Olympus BHS microscope with the microscope light-collimating lens moved as far from the objective lens as possible. Images are captured using a Nikon D1 digital camera. A Glass microscope micrometer is used to calibrate the spatial distances of the images. The approximate resolution of the images is 1 μm/pixel. Images will typically show a distinct bimodal distribution in the intensity histogram corresponding to the filaments and the background. Camera adjustments or different basis weights are used to achieve an acceptable bimodal distribution. Typically ten images per sample are taken and the image analysis results averaged.

The images are analyzed in a similar manner to that described by B. Pourdeyhimi, R. and R. Dent in “Measuring fiber diameter distribution in nonwovens” (Textile Res. J. 69(4) 233-236, 1999). Digital images are analyzed by computer using the MATLAB (Version. 6.1) and the MATLAB Image Processing Tool Box (Version 3—MathWorks, Natick, MA). The image is first converted into a grayscale. The image is then binarized into black and white pixels using a threshold value that minimizes the intraclass variance of the thresholded black and white pixels. Once the image has been binarized, the image is skeltonized to locate the center of each fiber in the image. The distance transform of the binarized image is also computed. The scalar product of the skeltonized image and the distance map provides an image whose pixel intensity is either zero or the radius of the fiber at that location. Pixels within one radius of the junction between two overlapping fibers are not counted if the distance they represent is smaller than the radius of the junction. The remaining pixels are then used to compute a length-weighted histogram of filament diameters contained in the image.

Kajaani FiberLab Fiber Analyzer SubTest Method Instrument Start-Up:

    • 1. Turn on Kajaani FiberLab Fiber Analyzer unit first, then computer and monitor.
    • 2. Start FiberLab program on computer.

Instrument Operation:

    • 1. File→New (or click on New File icon)
    • 2. “New Fiber Analysis” screen pops up.
      • a. Sample Point: select the folder you would like data stored in (to add a new folder see “Adding a New Folder”
      • b. Name: add condition or sample name/identifier here
      • c. Date
      • d. Time
      • e. Sample Weight: mg of dry fiber in the 50 ml sample (can leave blank if NOT measuring for coarseness). This is the number calculated in #10 of Sample Prep below.
    • 3. Make sure 50 ml of sample is placed in a “Kajaani beaker” and click “Start”
    • 4. Optional: Distribution→Measured Values
      • a. Fibers: the final count of measured fibers should be at least 10,000
      • b. Fibers/sec: this number must stay below 70 fibers/sec or the sample will automatically be diluted. If the sample is diluted during an analysis, the coarseness value will be invalid and will need to be discarded.
    • 5. A bar indicating the measurement status of a sample appears on the computer monitor. Do not start an analysis until the indicated status is “Wait State”. When the analysis is completed, wait for “Wait State” to appear, then close the “New Fiber Analysis” window. You can now repeat #1-3/4
    • 6. When finished with all samples, close the FiberLab program before turning off the Kajaani FiberLab analyzer unit.
    • 7. Shutdown computer.

Sample Preparation: Target Sample Size:

    • Softwood: 4 mg/50 m→160 mg BD in 2000 ml (~170-175 mg from sheet)
    • Hardwood: 1 mg/50 ml→40 mg BD in 2000 ml (~40-45 mg from sheet)
    • 1. For n=3 analysis, weigh and record weight of sample torn (avoiding cut edges) from 3 different pulp sheets of same sample using guidelines above for sample size. Place weighed samples into a suitable container for soaking of pulp.
    • 2. Using the 3 sheets that samples were torn from, perform moisture content analysis. Note: This step can be skipped if coarseness measurement is not required.
    • 3. Calculate the actual bone dry weight of the samples weighed in #1, by using the average moisture determined in #2.
    • 4. Allow pulp samples to soak in water for 10-15 minutes.
    • 5. Place 1st sample and soaking water into the Kajaani manual disintegrator. Fill disintegrator up to 250 ml mark with more water.
    • 6. Using the “hand dasher”, plunge up and down until sample is separated into individual fibers.
    • 7. Transfer sample to a 2000 ml volumetric flask. Make sure to wash off and collect any fibers that may have adhered to the dasher.
    • 8. Dilute up to 2000 ml mark. It is important to be as precise as possible for repeatable coarseness results.
    • 9. Take a 50 ml aliquot and place into a Kajaani beaker. Place beaker on the sampler unit.
    • 10. Calculate the mg of BD pulp in 50 ml aliquot
      • a. (BD mg of sample/2000 ml)×50 ml
    • 11. Begin Step #1 above in Instrument Operation

The water used in this method is City of Cincinnati Water or equivalent having the following properties: Total Hardness=155 mg/L as CaCO3; Calcium content=33.2 mg/L; Magnesium content=17.5 mg/L; Phosphate content=0.0462

Adding a New Folder to Sample Point Menu:

    • 1. Settings→Common Settings→Sample Folders
      • a. Type in name of new folder→Add→OK
    • Note: You must close the FiberLab program and re-open program to see the new folder appear in the menu.

Collecting Data in Excel File:

    • 1. Start FiberLab's Collect 1.12 program.
    • 2. Open Windows Explorer (not to full screen—you must be able to see both the Explorer and the Collect windows.
    • 3. In Windows Explorer . . . Select folder that data was stored in
    • 4. Highlight data to be put in Excel→right click on Copy→drag highlighted samples to the Collect window→Save text
    • 5. Click “Save In” menu bar and select “My briefcase”. Open the 2007 folder, type in file name and click Save. A message will appear saying the selected samples have been saved. Click OK (the sample names will disappear from the Collect window.
    • 6. Open Excel. Then . . . Open→Look In “My Briefcase”→2007→ at bottom, select “All Files (*.*)” in the “Files of Type” bar→find text file just saved and open→click thru the Text Import Wizard screens (next, next, finish)

Emtec Test Method

TS7 and TS750 values are measured using an EMTEC Tissue Softness Analyzer (“Emtec TSA”) (Emtec Electronic GmbH, Leipzig, Germany) interfaced with a computer running Emtec TSA software (version 3.19 or equivalent). According to Emtec, the TS7 value correlates with the real material softness, while the TS750 value correlates with the felt smoothness/roughness of the material. The Emtec TSA comprises a rotor with vertical blades which rotate on the test sample at a defined and calibrated rotational speed (set by manufacturer) and contact force of 100 mN. Contact between the vertical blades and the test piece creates vibrations, which create sound that is recorded by a microphone within the instrument. The recorded sound file is then analyzed by the Emtec TSA software. The sample preparation, instrument operation and testing procedures are performed according the instrument manufacture's specifications.

Sample Preparation

Test samples are prepared by cutting square or circular samples from a finished product. Test samples are cut to a length and width (or diameter if circular) of no less than about 90 mm, and no greater than about 120 mm, in any of these dimensions, to ensure the sample can be clamped into the TSA instrument properly. Test samples are selected to avoid perforations, creases or folds within the testing region. Prepare 8 substantially similar replicate samples for testing. Equilibrate all samples at TAPPI standard temperature and relative humidity conditions (23 °C±2 C° and 50%±2%) for at least 1 hour prior to conducting the TSA testing, which is also conducted under TAPPI conditions.

Testing Procedure

Calibrate the instrument according to the manufacturer's instructions using the 1-point calibration method with Emtec reference standards (“ref.2 samples”). If these reference samples are no longer available, use the appropriate reference samples provided by the manufacturer. Calibrate the instrument according to the manufacturer's recommendation and instruction, so that the results will be comparable to those obtained when using the 1-point calibration method with Emtec reference standards (“ref.2 samples”).

Mount the test sample into the instrument and perform the test according to the manufacturer's instructions. When complete, the software displays values for TS7 and TS750. Record each of these values to the nearest 0.01 dB V2 rms. The test piece is then removed from the instrument and discarded. This testing is performed individually on the top surface (outer facing surface of a rolled product) of four of the replicate samples, and on the bottom surface (inner facing surface of a rolled product) of the other four replicate samples.

The four test result values for TS7 and TS750 from the top surface are averaged (using a simple numerical average); the same is done for the four test result values for TS7 and TS750 from the bottom surface. Report the individual average values of TS7 and TS750 for both the top and bottom surfaces on a particular test sample to the nearest 0.01 dB V2 rms. Additionally, average together all eight test value results for TS7 and TS750, and report the overall average values for TS7 and TS750 on a particular test sample to the nearest 0.01 dB V2 rms.

Crystallinity Test Method—Differential Scanning Calorimetry

The equipment and materials used for this method are:

    • Differential Scanning calorimeter (DSC): TA Instruments Discovery 1 DSC with RCS chiller
    • DSC Firmware: 5.7.0.14
    • Control/analysis software: Trios, Version 5.0.0.44608
    • Pan: TA Instruments Tzero aluminum Pan Catalog #: T 141020.
    • Lid: TA Instruments Tzero Hermetic Lid Catalog #: T 240408
    • Biopsy punch: Integra Miltex 4 mm disposable biopsy punch
    • Balance: Mettler Toledo AB135-S/FACT Calibrated biyearly

Samples were stored in plastic bags at room temperature. For each sample repetition, a new Tzero pan and lid were tared and weight recorded. Using a 4 mm biopsy punch, a circle of web was punched out and placed in the pan. Sample size was between 15-18 mg. The sample weight was measured and recorded using a MT balance accurate to 0.01 mg (calibrated bi-yearly). The pan/lid was sealed using a TA Instrument pan crimper with corresponding Tzero crimping tools. Samples were run in triplicate. The pans were loaded into the DSC autosampler and ran in sequence using an empty Tzero pan/lid as reference. The DSC oven was purged with 50 m1/min nitrogen gas. The loading oven temperature was set to 25 °C. The experiment temperature profile was as follows:

    • Initial temp: 25 °C
    • Heat Ramp at 5 °C/min from 25 °C to 230 °C

Percent crystallinity was calculated from the integral of the melting peak (J/g) divided by the heat of fusion of fully crystallized PVOH (161.4 J/g)1 The average of the three repetitions is reported.

Cold Water Solubility Test Method

Fill a 2 L beaker with 1000 g of 25 °C deionized water and add 1.0 g of a melt blown PVOH web. Stir for 2 hours using a magnetic stir bar. After 2 hours, but while the mixture is still stirring, transfer four drops of the PVOH and water mixture to a microscope slide. This will ensure that no small, undissolved PVOH will settle to the bottom of the beaker. Place the slide on the stage of an optical microscope (VHX-5000 Keyence digital microscope). Using the 200× objective lens, focus the image to any debris in solution. Scan across the four drop sample of aqueous PVOH mixture using the XY stage and optically inspect for any residual fiber microstructure. Residual fiber microstructure includes individual fibers and/or fiber pieces that are not dissolved and/or partially dissolved fiber or fiber pieces that are swollen with water. If no residual fiber microstructure is optically detected the sample is considered cold water soluble.

Biodegradation Test Method

The biodegradability of the PVOH filaments was determined following the OECD 301B Ready Biodegradability CO2 Evolution Test Guideline. In this study, the test substance is the sole carbon and energy source and under aerobic conditions microorganisms metabolize the test substance producing CO2 or incorporating the carbon into biomass. The amount of CO2 produced by the test substance (corrected for the CO2 evolved by the blank inoculum) is expressed as a percentage of the theoretical amount of CO2 (ThCO2) that could have been produced if the organic carbon in the test substance was completely converted to CO2. Test substances achieving 60% of TCO2 within 10 days of reaching 10% TCO2 are regarded as readily biodegradable.

Surface Topography Test Method

In the Surface Topography Test the areal surface topology of a sample surface is measured using optical profilometry. The three-dimensional (3D) surface data are then processed and analyzed to extract the microscale areal surface texture parameter Sa (arithmetical mean height). Sa is the average value of the absolute value of height each point in the defined area, see FIG. 9.

3D surface topography images of the belts are obtained using high-intensity, LEDs in projection units on the Keyence VR-6000/6200 3D Optical Profilometer (Keyence Corporation of America, Itasca, IL). The system includes the following main components: a) a controller (VR-6000) which houses the high-intensity LED light source used for observation, control circuit boards, and other hardware and b) the head which is the unit that consists of the high-intensity LED light source for measurement, the CMOS camera, the scan optics, and the telecentric lens. Fringe projection light passes through the telecentric projection lens and impinges on the object diagonally from above. When there are height differences on the object surface and when light is applied to the object diagonally, the fringe projection image becomes distorted. The VR-6000 Series captures the distorted fringe projection image from straight above with the camera and measures the object height from the distortion.

The samples were placed flat on the motorized stage beneath the camera in ambient conditions, (20 °C to 25 °C and 20% to 30% RH). Two weights (about 17 g each) were placed on the sample outside of the measurement area to remove large scale waviness in the sample. Images were pre-processed before measurements following the instrument manufacturer's recommended procedures to correct for surface shape and noise. Regions of interest comprising of the microstructures on the CPN belts with overlaid PVOH fibers within the filtered height images were used to measure Sa, Sq, Ssk, Sku and Spd in accordance with ISO 25178-2:2012, see FIG. 9.

Ply Bond Test Method

The intent of this method is to reproducibly determine the strength to separate the plies between a layer of extruded fibrous elements, for example PVOH spun filaments, and one or more layers of web material.

The ply bond strength between a top extruded fibrous element layer and web material is measured using a tensile tester by pulling the plies apart in the machine direction for a pre-test distance of one inch and a test distance of four inches using four inch wide grips and a one inch gauge length.

The method is applicable to the measurement of material that is composed of a layer of extruded fibrous elements on top of one or more layers of web material.

Apparatus Conditioned Temperature and humidity controlled within the Room following limits: Temperature: 73 ± 2 °F (23 ± 1 °C) Relative Humidity: 50 ± 2% Tensile Tester General air operated grips (Cat No. #734 K, Grips recommended) with 1 inch (25.4 mm) by 4 inch (101.6 mm) inserts, or using the light weight upper grip assembly (Cat. No. 733-3012). Thwing-Albert Instrument Co., West Berlin, NJ. Tensile Tester EJA Vantage Tensile Tester (Thwing-Albert Instrument Co.). Calibration Laboratory weights certified by vendor Weights Ruler Ruler to check gauge length, 6 inch (152.4 mm) metal, with 0.01 inch (0.25 mm) graduations. Cat. # C305R-6, L. S. Starrett Co., Athol, MA 01331, or equivalent.

Sample Preparation

For this method, a usable unit is described as one sample prepared from an unconverted product or one finished product unit.

Converted Product

Condition the samples or useable units of product, with wrapper or packaging materials removed. Do not use samples from paper with obvious defects such as creases, tears, holes, etc. If the samples selected have defects of this kind, making them unsuitable for testing, discard. Replace with another sample which is free of such defects, selecting the replacement sample according to the product sampling plan. The sample is rolled out on a flat surface no more than two layers. High in a room conditioned at 50±2% relative humidity, 23 °C±1 °C for ten minutes prior to testing.

Discard the first ten usable sheets of the roll. After this, carefully remove singly from the roll the following sheets, 1, 2, 21, 22, 41, 42, 61, 62 (or the two consecutive sheets, i.e. 1, 2, can be removed together and separated later). Sheets 1, 21, 41, 61 will be used for initial testing purposes.

Sheets 2, 22, 42, 62 are retained for use as retest samples, and can be discarded if not used. Retests should only be performed in the event that during the ply separation process, the sample is damaged, torn, or made unsuitable for testing, the unsuitable sample should be discarded and the corresponding retest sample (Sheets 2, 22, 42, 62) should be used in its place. Separate the stacks of sheets for testing (sheets 1, 21, 41, 61) and retesting (sheets 2, 22, 42, 62) in the machine direction (in the order sheets come off the roll) with sides aligned. This results in one sample with 4 replicates. Each subsequent sample must be taken from a separate roll repeating the steps above.

Note: If a retest is needed, then retest the corresponding pair instead of the entire sample set.

Keep handling of the samples to a minimum. See FIG. 10.

Unconverted Product

The sample will be rolled out on a flat surface no more than two layers of unconverted product high in a room conditioned at 50±2% relative humidity, 23 °C±1 °C for ten minutes prior to testing. Do not use samples from paper with obvious defects such as creases, tears, holes, etc. If the samples selected have defects of this kind, making them unsuitable for testing, discard. Replace with another sample which is free of such defects, selecting the replacement sample according to the product sampling plan.

Taking from the center of the web, cut at least four samples that are 4″×4″ using a paper cutter with a built-in ruler to ensure the samples are dimensionally accurate. Note which direction in the sample is the machine direction when preparing the sample.

When testing, use a pair of forceps or tweezers and carefully separate the extruded fibrous element layer (spun layer) from the web material by inserting the tips at one end of the sample in the machine direction and prying them apart. Working your way across the cross direction of the sample, fully separate one inch of spun layer at the end of the sample and mount that spun layer into the top clamp of the tensile tester. Place the web material in the bottom of the clamp, see FIG. 11 for Ply Separation Diagram-Straight Perforation and FIG. 12 for Ply Separation Diagram-Shaped Perforation.

Alternatively, you may use Scotch tape and adhere a single layer of tape to the end of the sample with the length of the tape in the cross direction. This tape can help keep the layers together during separation.

If, during preparation or loading, the extruded fibrous element layer tears or is not able to be removed from the web material, discard the sample and cut a new one.

Start Up Procedures for Tensile Tester Software

    • 1. Ensure the computer is turned on.
    • 2. Select the MAP program icon on the desktop to launch the map software.
    • 3. Click on the folder icon in the upper left hand corner of the screen.
    • 4. Select the downward arrow located to the right of the LOOK IN box.
    • 5. Select the SCRIPT folder.
    • 6. Select the correct test script
    • 7. Select the (REAL TIME DATA) tab in the MAP program.
    • 8. Select the Position button in the lower right hand corner of the MAP program.
    • 9. Click on the Zero Load button to zero the load cell.
    • 10. Verify calibration of the tensile tester using calibrated weights.
    • 11. Ensure that the gauge length is 1 inch (25.4 mm), using a steel rule.
    • 12. Select the (FILES) tab in the MAP program.
    • 13. Name the data file.
    • 14. Click the REAL TIME DATA TAB to bring up the test window.

Operation

    • 1. Zero the instrument until the load cell reads 0 g+/−1.0 g. The load cell must read 0 g+/−1.0 g before each test.
    • 2. Clamp one of the separated plies into the upper grip and the other into the lower grip with the tail towards the analyst. Make sure the sample is centered in the grips and straight.
    • 3. Begin the test by depressing the start (i.e. test) button.
    • 4. Once the test is complete, remove the tested sample from the grips and discard.
    • 5. Repeat this procedure until all samples have been tested, making sure the load cell reads 0 g+/−1.0 g before each test.
    • 6. At any time during the test, if the sample completely separates then the data is invalid.

Calculations

The EJA Vantage tensile tester provides the calculated values of Load Mean, Standard Deviation and High Load.

The EJA Vantage tensile tester can also normalize the Load Mean and High Load values to the product width (label value sheet width) by taking the results and dividing them by the product width (label value sheet width). This calculation results in the data being expressed as grams per inches rather than grams per sheet.

Two-Ply Tissue Average Ply Bond Strength (four replicates per sample): Load Mean (g) Sum of Load Means (g) Average Ply Bond = Number of two-ply toilet tissue usable units tested (four reps)

Unconverted Sample Average Ply Bond Strength (four replicates per sample): Load Mean (g) Sum of Load Means (g) Average Ply Bond = Number usable units tested (four reps) Note: four reps per ply separation

Reporting Results

Report the Load Mean results to the nearest 0.1 gram per sheet.

Tensile

Samples for tensile strength testing are prepared by cutting a 3″ (76.2 mm)×5″ (127 mm) long strip in either the machine direction (MD) or cross-machine direction (CD) orientation using a JDC Precision Sample Cutter (Thwing-Albert Instrument Company, West Berlin, NJ, Model No. JDC 3-10, Ser. No. 37333). The instrument used for measuring tensile strengths is an MTS Systems Sintech 11S, Serial No. 6233. The data acquisition software is MTS TestWorks™ for Windows Ver. 4 (MTS Systems Corp., Research Triangle Park, N.C.). The load cell is selected from either a 50 or 100 Newton maximum, depending on the strength of the sample being tested, such that the majority of peak load values fall between 10 and 90 percent of the load cell's full scale value. The gauge length between jaws is 2±0.04 inches (50.8±1 mm). The jaws are operated using pneumatic-action and are rubber coated. The minimum grip face width is 3″ (76.2 mm), and the approximate height of a jaw is 0.5 inches (12.7 mm). The crosshead speed is 10±0.4 inches/min (254±1 mm/min), and the break sensitivity is set at 65 percent. The sample is placed in the jaws of the instrument, centered both vertically and horizontally. The test is then started and ends when the specimen breaks. The peak load is recorded as either the “MD tensile strength” or the “CD tensile strength” of the specimen depending on the sample being tested. At least six (6) representative specimens are tested for each product, taken “as is,” and the arithmetic average of all individual specimen tests is either the MD or CD tensile strength for the product.

Filament Moisture Content

A stainless-steel, perforated insert that is cut to approximately 3.5 inches in diameter is placed in an aluminum weight pan and tared on a gravimetric moisture analyzer (Mettler Toledo, Model: HB4-S). The stainless-steel insert is then grasped with long reach needle-nosed pliers and laid on top of a wet laid substrate that is being unwound onto a forming belt.

Using the long reach needle-nosed pliers to hold the stainless-steel on top of the wet laid paper which is being unwound on a forming belt, the insert is passed underneath the melt blown die until 0.5 g to 2.0 g of filament material is collected. Quickly, place the insert with spun filaments in the aluminum weighing pan that is in the moisture analyzer. Close the lid of the analyzer and heat the sample to 200 °C using the Rapid Heat function on the Mettler Toledo HB43-S. Record the % water of the sample when the heating cycle ends. Repeat this measurement five times and average the % water content for reporting.

Pilling Test Method

The pilling property of toilet tissue and facial tissue is measured quantitatively with a Sutherland Ink Rub Tester and flatbed scanner. The rub tester is a motor driven instrument, which rubs or moves a weight with an attached black felt pad over a stationary tissue sample for precisely 3 strokes. The black felts are placed on the flatbed scanner and are analyzed using MATLAB software.

This method applies to finished tissue product and unconverted stock. The number of plies does not influence the results.

Apparatus Conditioned Room Temperature and humidity controlled within the following limits: Temperature: . . . 73° ± 2 °F (23° ± 1 °C) Relative humidity: . . . 50% ± 2% Rub Tester Sutherland Ink Rub Tester- Cam A Special (old style cam with longer stroke; Danilee Co., LLC, Medina, OH). A scoring device and a five-pound weight are included. It has four square inches of effective contact area which provides a contact pressure of 1.25 pounds per square inch Flatbed Scanner Fujitsu model fi-60, part number PA03595-B005, or equivalent (Fujitsu Computer Products of America, Inc. Sunnyvale, CA). Software Matlab R2014 or newer from MathWorks, Natick, MA, Cellophane Tape Any convenient source (e.g. Scotch tape), width ¾ inch (19.2 mm). Book Tape 2 inch (50.8 mm) 3M # 845 Double-Sided Tape 2 inch (50.8 mm) 3M # 9589 Rubber Pads Closed Cell Neoprene Sponge ⅛″ thick Alfa Cutter Catalog No. 240-7A or Catalog 240-7B or Catalog No. 240-10 (recommended); Thwing-Albert Instrument Co. Berlin, NJ, or equivalent. Paper Cutter Convenient Source, 12 inch × 15 inch or larger Cutting Dies 4.75 (MD) × 5.0 in (CD). (114.3 × 127 mm), area precision: less than 0.2%, WDS, Harrison, Ohio. Die must be modified with soft foam rubber insert material. Illustration Board Crescent # 300 “Cardboard” Canned Air 8 oz. Pressurized Dust-Off or equivalent. If available facility compressed with tube and air gun can be used. Black Felt F55 Black Felt 75% Needled Wool, 2 mm thick. Obtained from Superior Felt

General Instructions

These instructions are for the preparation of a single sample-one side only. If both sides (for example, both embossed and non-embossed side or non-cellulose and cellulose side) are requested repeat this procedure for other side using a fresh sample. Repeat this procedure for all replicates. The rub tester base and the five-pound rub tester weight use 6×2½ in. (152×63.5 mm) rubber pads.

Preparation of Rubber Pad Material

Using the paper cutter, trim a needed amount (6×2½ in) of rubber pad material so it has straight edges on all sides.

Raise the corner of the pad material up from the very bottom corner of the cutter so that when the cutting blade is lowered it will not shear the material.

Line up with the cut edges and place double-sided tape #9589 to one side of the trimmed pad material. Cut the tape as needed with scissors to the pad dimensions.

Remove the backing on the double-sided tape, align the pad with tape side down, and place the pad on rub tester on the testing area. Cut a second pad and apply it to the five pound weight.

Preparation of Sample and Felt Card

Using a paper cutter, cut illustration board into 2½×6±⅛ in. sample cards. Prepare as many cards as needed. For sample cards that will be used on rub testers equipped with holding pins, puncture two holes in each card by forcing the cardboard onto the pins or predrill the holes to fit snuggly over the pins.

Application of Book Tape on Sample Card

Cut a 4-in. piece of book tape. Align the tape with the top end of the card and attach centered within the card area. Wrap the tape so that the entire top 2-in. is sealed with tape.

Ensure tape is securely attached to the card by rubbing firmly.

Place book tape on the bottom end of the card in a similar manner.

Sample Preparation

For this method, a usable unit is described as one finished product unit regardless of the number of plies. Samples and black felts are conditioned with all wrapping or packaging materials removed in the controlled temperature and humidity room. Samples are to be conditioned for a minimum of ten minutes with no more than 2 layers. Black felt is thicker than the samples being measured and does not equilibrate in ten minutes, therefore the conditioning time will remain 2 hours (Black Felt only).

Finished Product

For new samples, discard at least 15 usable units from the roll or several usable units from the carton. Use only usable units free of holes, tears, wrinkles, and other defects.

One, Two, and Three Ply Toilet Tissue

Remove a strip of toilet tissue three usable units long. Separate the units by carefully separating at the perforations.

Stack and align three units for testing with the perforations at the top of the sample. The units should all be aligned in the machine direction and the outer sides facing the same direction.

Unconverted Stock

Cut into the reel or sample stack several plies deep to obtain a representative sample for testing. Using a paper cutter cut three strips 4.75 in.×5 in. with the 4.75 in. dimension running in the machine direction. Alternatively, an Alfa cutter with a correctly sized die can be used to cut the samples. For tissue containing specialty fibers which are primarily located on just one side, testing may be limited to the specialty side.

Flip the sample stacks so that the side to be tested is down. Center a sample card on the stack with the 6-in. card dimension parallel to the machine direction of the sample.

Carefully flip the sample stacks so that the sample card is down. Apply masking tape across the top and bottom of the stack. Each strip of tape should wrap around and attach to the back side of the card. The sample should be snug on the card but be careful to not stretch or tear. If stretching or tearing occurs prepare another sample.

Operation

Set up the Sutherland Rub Tester according to the manufacturer's instructions. For this method, the tester is preset for three strokes and operates at Sutherland standard speed 2 (approximately 42 cycles per minute). A stroke is defined as one complete back and forth motion. Ensure the instrument is delivering the correct number of strokes by starting the tester and counting. Monitor the stroke count frequently during testing.

Place the weight so that the pad side is up. Center a felt on the pad and secure both ends with the available weight clamps.

Place a prepared sample card on the base plate of the rub tester.

Hook the weight onto the tester arm and gently lower onto the prepared sample card. Use a level to ensure the block does not lean on the felt.

It is important to check that the felt rests flat on the sample and that the weight does not bind on the arm.

Start the rub tester and at the end of three complete strokes remove the weight from the tester arm. If the tissue sample is intact or only slightly torn, carefully remove the rubbed felt from the weight clamps.

Calculations

The image is acquired as an 8-bit gray scale 4×6 inch image at 600 dots per inch yielding an image that is 2400×3600 pixels in size. The left inch and right inch of this image (see the Figure below) contains a gray scale calibration scale (Kodak Color Separation and Gray Scale (Small) Cat #152 7654). The gray scale strip is attached to a scanner bracket that centers the sample on the scanner. The center 2 inches of the image contains the image of the rubbed felt. The bottom inch of the image contains unrubbed felt. The remaining area contains the rubbed area of interest. This area is cropped from the total image and processed. The steps include;

    • 1. A section of the gray scale (gray scale step 14) is cropped from the image and the average value in this cropped image is used as a thresholding value. A typical value for the threshold is 43±1.
    • 2. The processed area is then thresholded in MATLAB using the above calculated threshold value. This creates a black and white image where any pixel with a higher gray value than the threshold value is given a value of one and any pixel with a lower gray value than the threshold value is given a value of zero.
    • 3. The custom MATLAB program takes this binary image and identifies groups of connected white pixels as separate objects. It then measures the size of each object by calculating its equivalent diameter, which is halved to get the radius. Finally, it uses these radii to determine the volume of each object.
    • 4. The equivalent volumes are binned by size, are counted, and the bins are summed to calculate total volume in each bin. The bins are;
      • a. Anything volume greater than 100 mm3.
      • b. Volumes greater than 50 but less than 100 mm3.
      • c. Volumes greater than 10 but less than 50 mm3.
      • d. Volumes greater than 1 but less than 10 mm3.
      • e. Any volume less than 1 mm3.

The reported pilling value (Total Pilling Volume) is the sum of all the volumes above in Step 4. bins a.-e.

Glide Test Method—3 Inch Sample

This test is designed to measure the adhesive characteristics between two different surfaces of a fibrous structure, for example toilet tissue (Dual Surface Glide Value) and a single surface of a fibrous structure, for example toilet tissue (Single Surface Glide Value).

One objective of this Glide Test Method is to quantify the Peak Load and Drag Force required for one surface in a fibrous structure, for example toilet tissue, such as a surface material surface, to move across a different surface in the fibrous structure, for example toilet tissue, such as a web material surface, referred to as Dual Surface Glide Value.

Another objective of this Glide Test Method is to quantify the Peak load and Drag force required for one surface in a fibrous structure, for example toilet tissue to move across the same surface in the fibrous structure, for example toilet tissue, such as a surface material surface, referred to as Single Surface Glide Value.

As shown in FIG. 15 the Drag Force is determined by pulling about a 3″ wide×12″ long strip of a fibrous structure, for example a toilet tissue with a first surface over a different surface of about a 3″ wide×16″ long strip of the same fibrous structure, for example the same toilet tissue using a friction/peel tester.

This method is intended for use on toilet tissue and unconverted fibrous structure stock.

Friction/Peel Thwing-Albert FP-2260 Friction/Peel Tester, 2000 g Tester 2000 load cell 2002 Sampling Rate 60 Hz Loadcell Mode Tension Loadcell Range 100% Pre-Test Load 3 g Return Speed 1000 mm/min Test Speed 60 mm/min Software MAP 4, Version 4.3.12 or later Tape Scotch 1″ Tape, or equivalent Conditioned Temperature and humidity controlled within the Room following limits: For Laboratory: Temperature: 73 °F ± 2 °F (23 °C ± 1 °C) Relative humidity: 50% (±2%) Sample Cutter Scissors Paper Cutter Cutting Board, 24 in size String 2004 Ultracast Spiderwire 20 1b 0.0009″ diameter Metal Roller Solid Aluminum Roll, 1⅞″ diameter, 5⅛″ long, 2006 615 g mass Binder Clip ¾″ Wide 2008

Sample Preparation

For this method, a sample of the fibrous structure, for example toilet tissue for testing may have one or more plies.

Condition the sample(s) with any wrapping or packaging material removed for a minimum of two hours in a room conditioned at 50% RH±2% and 73 °F±2 °F. Do not use samples from paper with obvious defects such as creases, tears, holes, etc.

For Toilet Tissue, for example single- or multi-ply toilet tissue roll:

Remove the outer 8-10 useable units from the toilet tissue roll to prevent testing materials that have been “handled.” Then, carefully remove one strip of useable units from the toilet tissue roll such that about a 3″ wide×16″ long strip of toilet tissue is able to be cut from the strip of useable units. As shown in FIG. 15 cut about a 3″ wide×16″ long sample strip 2010 from the strip of useable units and place the sample strip 2010 on the surface 2012 of the sled of the Friction/Peel Tester 2000 with the outer side of the sample strip 2010 (consumer-contacting surface) facing up. Clamp one end of the sample strip 2010 using the built-in clamp 2014 at the beginning of the sled surface 2012.

For the Dual Surface Glide Value measurement, remove another strip of useable units from the same toilet tissue roll such that about a 3″ wide×12″ long strip of toilet tissue is able to be cut from the strip of useable units. Cut about a 3″ wide×12″ long sample strip 2016 from the strip of useable units and place the sample strip 2016 on top of the previously positioned sample strip 2010 already lying on the surface 2012 of the sled of the Friction/Peel Tester 2000 ensuring that the edges 2018 of both of the sample strips 2010 and 2016 line up perfectly (or as perfectly as possible in the case of product defects). The end of the top sample strip 2016 should be approximately one inch away from the built-in clamp 2014.

For the Dual Surface Glide Value measurement, the sample strips 2010 and 2016 are arranged such that different surfaces of the toilet tissue are in contact with one another for the test.

For the Single Surface Glide Value measurement, the sample strips are arranged such that the surfaces of the toilet tissue in contact with each other are the same.

Unconverted Stock:

To create the sample strip for clamping to the built-in clamp 2014 of the sled surface 2012 of the Fiction/Peel Tester, cut a stack (no more than 5 fibrous structures thick) of unconverted stock into strips of 16″ long in the Machine Direction and 3″ in the Cross Machine Direction. To create the sample strip for testing, cut a stack (no more than 5 fibrous structures thick) of unconverted stock into strips of 12″ long in the Machine Direction and 3″ in the Cross Machine Direction.

Place the sample strip for clamping on the built-in clamp (16″ long in the Machine Direction) with the consumer-contacting surface, for example surface material surface facing up so that the machine direction faces left to right on the Friction/Peel Tester sled surface. Clamp this sample strip at the left side of the sled underneath the built-in clamp. Place the sample strip for testing (12″ long in the Machine Direction) on top of the previously positioned sample strip already lying on the surface of the sled of the Friction/Peel Tester ensuring that the edges of both of the sample strips line up perfectly (or as perfectly as possible in the case of product defects). The end of the top sample strip should be approximately one inch away from the built-in clamp.

For the Dual Surface Glide Value measurement, the sample strips are arranged such that different surfaces of the unconverted stock are in contact with one another for the test. For the Single Surface

Glide Value measurement, the sample strips are arranged such that the surfaces of the unconverted stock in contact with each other are the same.

Operation

Using a length of string 2004, for example Spiderwire line, loop the string 2004 through one of the “eyes” 2020 of the binder clip 2008 and through the probe 2022 of the load cell 2002. Tie off the string 2004 so that the total length of the loop is 1″ while the loop holds the binder clip 2008 to the probe 2022 of the load cell 2002. Gently set the binder clip 2008, now tied to the probe 2022, so that the binder clip 2008 gently rests on the load cell 2002 (not the probe 2022) so that the string 2004 that holds the binder clip 2008 is completely slack. Zero the load cell 2002.

Move the crosshead 2024 towards the built-in clamp 2014 so that the binder clip 2008 may attach to the right end of the top sample strip 2016 without pulling on the probe 2022 (the string 2004 is slack). If unconverted stock is being tested, tape the right edge of the top sample strip to prevent the sample strip from tearing if the static force may be stronger than the tensile force of the sample strip. If the sample strip tears, discard the data for the sample strip and repeat with a new sample strip.

Line up the sample strip 2016 so that the binder clip 2008, the probe 2022 tip, and the side closest to the built-in clamp 2014 of the sample strip 2016 all form a straight line and are “parallel” to one another. This is done to prevent the sample strip 2016 from being pulled at an angle, rather than along the length of the bottom sample strip 2010.

Gently position the metal roller 2006 at the left side of the top sample strip 2016 closest to the built-in clamp 2014. The bottom of the metal roller 2006 should not yet be on the top sample strip 2016. Roll the metal roller 2006 from left to right so that the metal roller 2006 comes to rest when it makes contact with the binder clip 2008, taking care not to press down on the metal roller 2006 during the rolling. The roll time of the metal roller 2006 should be 3-5 seconds from start to finish. Do not roll the metal roller 2006 back and forth over the sample strip 2016, as this will cause additional bonding. If obvious defects such as large wrinkles form, discard the sample strip and repeat the test with another sample strip.

Select the yellow “Pre-Test” button. This will pull the slack out of the string 2004 and add 3 g tension to the load cell 2002. Before proceeding, confirm that the probe 2022 tip, the eye 2020 of the binder clip 2008, and the middle of the sample strip 2016 all form a straight line as mentioned previously.

Begin the test. Monitor the Friction/Peel Tester 2000 for any signs of slippage from the binder clip 2008 when at high tensile force, especially when using tape. If slippage occurs, discard the data for the sample strip 2016 and repeat with a new sample strip 2016. When the test completes, the crosshead 2024 will move back to its home condition. To avoid any unintentional damage to the probe 2022, be sure to unclamp the sample strip 2016 and return the binder clip 2008 to the top of the load cell 2002 (or hold the binder clip 2008) until the crosshead 2024 stops moving.

Run a total of 5 replicates by repeating the entire test method each time.

Calculations

Peak Load=sum of max force readings/number of replicates tested; namely 5 replicates. Drag Force=average of the load cell values from the 20 mm point to the 40 mm point of the pulling distance, even though the sample strip is pulled a total of 40 mm. This Drag Force is reported in units of g to the nearest 0.1 g. The reported Dual Surface Glide Value and the Single Surface Glide Value are the average of their respective Drag Forces for 5 replicates and are reported in units of g to the nearest 0.1 g.

Glide Test Method—4 Inch Sample

This test is designed to measure the adhesive characteristics between two different surfaces of a fibrous structure, for example toilet tissue (Dual Surface Glide Value) and a single surface of a fibrous structure, for example toilet tissue (Single Surface Glide Value).

One objective of this Glide Test is to quantify the peak load and drag force required for the one surface in a fibrous structure, for example toilet tissue, such as a surface material surface, to move across a different surface in the fibrous structure, for example toilet tissue, such as a web material surface, referred to as Dual Surface Glide Value.

Another objective of this Glide Test is to quantify the peak load and drag force required for the one surface in a fibrous structure, for example toilet tissue to move across the same surface in the fibrous structure, for example toilet tissue, such as a surface material surface, referred to as Single Surface Glide Value.

As shown in FIG. 15 the drag force is determined by pulling about a 4″ wide×12″ long strip of a fibrous structure, for example a toilet tissue with a first surface over a different surface of about a 4″ wide×16″ long strip of the same fibrous structure, for example the same toilet tissue using a friction/peel tester.

This method is intended for use on toilet tissue and unconverted fibrous structure stock.

Friction/Peel Thwing-Albert FP-2260 Friction/Peel tester, 2000 g Tester 2000 load cell 2002 Sampling Rate 60 Hz Loadcell Mode Tension Loadcell Range 100% Pre-Test Load 3 g Return Speed 1000 mm/min Test Speed 60 mm/min Software MAP 4, Version 4.3.12 or later Tape Scotch 1″ Tape, or equivalent Conditioned Temperature and humidity controlled within Room the following limits: For Laboratory: Temperature: 73 °F ± 2 °F (23 °C ± 1 °C) Relative humidity: 50% (±2%) Sample Cutter Scissors, 4 in or larger Paper Cutter Cutting Board, 24 in size String 2004 Ultracast Spiderwire 20 1b 0.0009″ diameter Metal Roller Solid Aluminum Roll, 1⅞″ diameter, 5⅛″ long, 2006 615 g mass Binder Clip ¾″ Wide 2008

Sample Preparation

For this method, a sample of the fibrous structure, for example toilet tissue for testing may have one or more plies.

Condition the sample(s) with any wrapping or packaging material removed for a minimum of two hours in a room conditioned at 50% RH±2% and 73 °F±2 °F. Do not use samples from paper with obvious defects such as creases, tears, holes, etc.

For Toilet Tissue, for Example Single- or Multi-Ply Toilet Tissue Roll:

Remove the outer 8-10 useable units from the toilet tissue roll to prevent testing materials that have been “handled.” Then, carefully remove one strip of useable units from the toilet tissue roll such that about a 4″ wide×16″ long strip of toilet tissue is able to be cut from the strip of useable units. As shown in FIG. 15 cut about a 4″ wide×16″ long sample strip 2010 from the strip of useable units and place the sample strip 2010 on the surface 2012 of the sled of the Friction/Peel Tester 2000 with the outer side of the sample strip 2010 (consumer-contacting surface) facing up. Clamp one end of the sample strip 2010 using the built-in clamp 2014 at the beginning of the sled surface 2012.

For the Dual Surface Glide Value measurement, remove another strip of useable units from the same toilet tissue roll such that about a 4″ wide×12″ long strip of toilet tissue is able to be cut from the strip of useable units. Cut about a 4″ wide×12″ long sample strip 2016 from the strip of useable units and place the sample strip 2016 on top of the previously positioned sample strip 2010 already lying on the surface 2012 of the sled of the Friction/Peel Tester 2000 ensuring that the edges 2018 of both of the sample strips 2010 and 2016 line up perfectly (or as perfectly as possible in the case of product defects). The end of the top sample strip 2016 should be approximately one inch away from the built-in clamp 2014.

For the Dual Surface Glide Value measurement, the sample strips 2010 and 2016 are arranged such that different surfaces of the toilet tissue are in contact with one another for the test. For the Single Surface Glide Value measurement, the sample strips are arranged such that the surfaces of the toilet tissue in contact with each other are the same.

Unconverted Stock:

To create the sample strip for clamping to the built-in clamp 2014 of the sled surface 2012 of the Fiction/Peel Tester, cut a stack (no more than 5 fibrous structures thick) of unconverted stock into strips of 16″ long in the Machine Direction and 4″ in the Cross Machine Direction. To create the sample strip for testing, cut a stack (no more than 5 fibrous structures thick) of unconverted stock into strips of 12″ long in the Machine Direction and 4″ in the Cross Machine Direction.

Place the sample strip for clamping on the built-in clamp (16″ long in the Machine Direction) with the consumer-contacting surface, for example surface material surface facing up so that the machine direction faces left to right on the Friction/Peel Tester sled surface. Clamp this sample strip at the left side of the sled underneath the built-in clamp. Place the sample strip for testing (12″ long in the Machine Direction) on top of the previously positioned sample strip already lying on the surface of the sled of the Friction/Peel Tester ensuring that the edges of both of the sample strips line up perfectly (or as perfectly as possible in the case of product defects). The end of the top sample strip should be approximately one inch away from the built-in clamp.

For the Dual Surface Glide Value measurement, the sample strips are arranged such that different surfaces of the unconverted stock are in contact with one another for the test. For the Single Surface Glide Value measurement, the sample strips are arranged such that the surfaces of the unconverted stock in contact with each other are the same.

Operation

Using a length of string 2004, for example Spiderwire line, loop the string 2004 through one of the “eyes” 2020 of the binder clip 2008 and through the probe 2022 of the load cell 2002. Tie off the string 2004 so that the total length of the loop is 1″ while the loop holds the binder clip 2008 to the probe 2022 of the load cell 2002. Gently set the binder clip 2008, now tied to the probe 2022, so that the binder clip 2008 gently rests on the load cell 2002 (not the probe 2022) so that the string 2004 that holds the binder clip 2008 is completely slack. Zero the load cell 2002.

Move the crosshead 2024 towards the built-in clamp 2014 so that the binder clip 2008 may attach to the right end of the top sample strip 2016 without pulling on the probe 2022 (the string 2004 is slack). If unconverted stock is being tested, tape the right edge of the top sample strip to prevent the sample strip from tearing if the static force may be stronger than the tensile force of the sample strip. If the sample strip tears, discard the data for the sample strip and repeat with a new sample strip.

Line up the sample strip 2016 so that the binder clip 2008, the probe 2022 tip, and the side closest to the built-in clamp 2014 of the sample strip 2016 all form a straight line and are “parallel” to one another. This is done to prevent the sample strip 2016 from being pulled at an angle, rather than along the length of the bottom sample strip 2010.

Gently position the metal roller 2006 at the left side of the top sample strip 2016 closest to the built-in clamp 2014. The bottom of the metal roller 2006 should not yet be on the top sample strip 2016. Roll the metal roller 2006 from left to right so that the metal roller 2006 comes to rest when it makes contact with the binder clip 2008, taking care not to press down on the metal roller 2006 during the rolling. The roll time of the metal roller 2006 should be 3-5 seconds from start to finish. Do not roll the metal roller 2006 back and forth over the sample strip 2016, as this will cause additional bonding. If obvious defects such as large wrinkles form, discard the sample strip and repeat the test with another sample strip.

Select the yellow “Pre-Test” button. This will pull the slack out of the string 2004 and add 3 g tension to the load cell 2002. Before proceeding, confirm that the probe 2022 tip, the eye 2020 of the binder clip 2008, and the middle of the sample strip 2016 all form a straight line as mentioned previously.

Begin the test. Monitor the Friction/Peel Tester 2000 for any signs of slippage from the binder clip 2008 when at high tensile force, especially when using tape. If slippage occurs, discard the data for the sample strip 2016 and repeat with a new sample strip 2016. When the test completes, the crosshead 2024 will move back to its home condition. To avoid any unintentional damage to the probe 2022, be sure to unclamp the sample strip 2016 and return the binder clip 2008 to the top of the load cell 2002 (or hold the binder clip 2008) until the crosshead 2024 stops moving.

Run a total of 5 replicates by repeating the entire test method each time.

Calculations

    • Peak Load=sum of max force readings/number of replicates tested; namely 5 replicates.
    • Drag Force=average of the load cell values from the 20 mm point to the 40 mm point of the pulling distance, even though the sample strip is pulled a total of 40 mm. This Drag Force is reported in units of g to the nearest 0.1 g. The reported Dual Surface Glide Value and the Single Surface Glide Value are the average of their respective Drag Forces for 5 replicates and are reported in units of g to the nearest 0.1 g.

EXAMPLES Example 1

TABLE 1 Bonding, Drying, and Forming Centerlines and Resulting Softness and Pilling Drying Forming TS7 Drying Air Air (dB Thermal Temperature Flowrate Flowrate V2 Pilling Bond (C°) (m3/hr) (m3/hr) rms) (mm3) Sample 1 -Comparative Yes 232 1014 426 8.1 9,900 Sample 2 -Comparative No 232 1014 426 6.2 >10,000 Sample 3 -Inventive No 100 570 1020 6.7 8,700 Sample 4 -Comparative No 100 570 1020 6.5 >10,000 Sample 5 -Comparative Yes 100 570 1020 9.7 9,800 Sample 6 - Inventive No 100 570 1020 5.8 9,800

TABLE 1 compares the TS7 and pilling values of six Samples—a thermal bonded product, high drying and low forming (Comparative Sample 1), a completely unbonded product with no thermal bonding and no random bonding because the product was made at high drying and low forming centerlines (Comparative Sample 2), and a randomly bonded product made at low drying and high forming centerlines which results in a slightly tacky environment for the hydroxyl polymer filaments (Inventive Sample 3). The two Comparative Samples either have high TS7 or high pilling, while the Inventive Sample has the desired combination of low TS7 and low pilling that is preferred by consumers. Comparative Sample 4 is another comparative example which displays the importance of having the right level of fast wetting surfactant in the composition. If there is a relatively high level of fast wetting surfactant in the composition (3 wt %), as described in U.S. Pat. No. 10,696,821, the water was removed very quickly from the polysaccharide filament as it is attenuated which results in a high storage modulus at equivalent laydown conditions and the web does not become tacky to sufficiently adhere to the wet laid substrate resulting in very high pilling. Comparative Sample 5 is another comparative example which displays the undesirable surface feel of an overly bonded structure. In this example, the structure is both thermal bonded and randomly bonded via lower drying temperature and higher forming vacuums resulting in a relatively high TS7 value of 9.7 dB V2 rms. Inventive sample 6 shows the desired combination of TS7 and pilling when a randomly bonding a polysaccharide composition with a relatively low level of fast-wetting surfactant at 0.5 wt % relative to PVOH.

Sample 1—Comparative Sample—Thermal Bonded, High Drying and Low Forming

In a 40:1 APV Baker twin-screw extruder (Baker Perkins Co., Grand Rapids, MI) with eight temperature zones, 260 g/min of Purity Gum Ultra Food Starch Modified Corn Starch from Ingredion (Indianapolis, IN) and 53 g/min water were added to Zone 1, using the temperature profile shown in TABLE 2 below. This mixture was then conveyed down the barrel through zones 2 through 8 at a screw speed of 500 RPM, where a second water injection of 97 g/min was introduced at zone 6. After exiting the extruder, the material was a homogeneous, uniform melt-processed polysaccharide composition with a water content of 40%. The water content was determined by collecting a melt sample in a plastic syringe and then ejecting the melt sample from the syringe onto an aluminum weight dish. The dish was weighed before and after drying in an oven overnight at 110 °C to determine how much water was in the original sample. The extruder barrel temperature setpoints for each zone are shown below in TABLE 2.

TABLE 2 Zone 1 2 3 4 5 6 7 8 Temperature (°C) 16 49 81 93 93 93 121 121

The temperature of the melt exiting the 40:1 extruder is between 121 and 132 °C. The melt temperature was measured with an in-line thermocouple. From the extruder, the melt was fed to a Zenith gear pump, Model #60-20000-2366-4 (Zenith Precision Metering, Monroe, NC), and the pump metered the melt to two static mixers where an additional 179 g/min of water was added. The melt composition at this point in the process was 58% water and 42% polysaccharide. From the static mixers, the polysaccharide melt composition was pumped to a melt blowing spinneret via a melt pump (Zenith gear pump, Model 5 #60-20000-2366-4).

A plurality of polysaccharide filaments was attenuated with a steam saturated air stream at 74 °C and 88% relative humidity to form a layer of filaments between 1 and 2 gsm that was collected either directly onto a forming belt or onto a differential density wet laid cellulose structure with a micro pattern of knuckles and pillows. The fibers were formed in a relatively low RH environment of less than 20%, by drying them using air at 232 °C temperature and 1014 m3/hr flowrate. Furthermore, a low forming air flow of 426 m3/hr was employed to gently laydown the filaments on the underlying wet laid paper and to retain fiber loft and mobility. The water content of the spun filament layer was less than 1.0 wt % using the Filament Moisture Content Test Method. The ply bond strength between the layer of PVOH filaments and the wet laid cellulosic structure was relatively low at 9.7 g as measured by the Ply bond Test Method, because there is very little adhesion between the two layers. Consequently, the layered substrate was bonded with a high temperature, high pressure patterned nipped roll at 150 °C and 325 psi to sufficiently attach the layers together. The thermal bonded substrate was wound about a core to produce a parent roll.

This parent roll was unwound and combined and embossed with a wet-laid fibrous structure ply from a wet laid fibrous structure parent roll using glue to form a 2-ply embossed layered fibrous structure, such as a 2-ply toilet tissue product. A surface softener was then added from 5 to 20 lb/tne to the embossed side of the tissue product using a slot coater. The 2-ply toilet tissue product was wound and then tail sealed and cut to width to create a finished product roll of toilet tissue product. The resulting 2-ply toilet tissue product had a TS7 value of 8.1 dB V2 rms as measured by the Emtec Test Method, and a pilling value of less than 9,900 mm3 as measured by the Pilling Test Method.

Sample 2—Comparative Sample-Non Thermal Bonded, High Drying and Low Forming

A layered fibrous structure with a surface layer of polysaccharide filaments spun onto a wet laid cellulosic substrate was prepared similarly to Sample 1 except the layered fibrous structure was not bonded with a high temperature, high pressure thermal bond roll. The water content of the spun filament layer was 0.7 wt % using the Filament Moisture Content Test Method. The ply bond strength between the layer of PVOH filaments and the wet laid cellulosic structure is relatively low because there is very little adhesion between the two layers. After being combined and embossed with a wet-laid fibrous structure ply from a wet laid fibrous structure parent roll, the resulting 2-ply toilet tissue product has a TS7 value of 6.2 dB V2 rms as measured by the Emtec Test Method, and a pilling value greater than 10,000 mm3 as measured by the Pilling Test Method. The relatively high pilling result is because the PVOH spun layer was not adequately attached to the wet laid substrate.

Sample 3—Inventive Sample-Non Thermal Bonded and Random Bonded Via Tacky Laydown Conditions (Low Drying and High Forming)

A polysaccharide melt composition was prepared and pumped to a melt blowing die similarly to Sample 1. A plurality of polysaccharide filaments was attenuated with a steam saturated air stream at 74 °C and 88% relative humidity to form a layer of filaments between 1 and 2 gsm that is collected either directly onto a forming belt or onto a differential density wet laid cellulose structure with a micro pattern of knuckles and pillows. The fibers were formed in a relatively high RH environment by drying them using air at 100 °C temperature and 570 m3/hr flowrate. Furthermore, a high forming air flow rate of 1020 m3/hr was employed to create a negative pressure differential at the consumer facing outer surface of the substrate. The water content of the spun filament layer was 3.1 wt % using the Filament Moisture Content Test Method. The ply bond strength between the layer of PVOH filaments and the wet laid cellulosic structure was relatively high because there is good adhesion between the blended polysaccharide fibers and the wet laid substrate. The layered substrate was not bonded with a high temperature, high pressure patterned nipped roll and wound to produce a parent roll.

This parent roll was unwound and combined and embossed with a wet-laid fibrous structure ply from a wet laid fibrous structure parent roll using glue to form a 2-ply embossed layered fibrous structure, such as a 2-ply toilet tissue product. A surface softener was then added from 5 to 20 lb/tne to the embossed side of the tissue product using a slot coater. The 2-ply toilet tissue product was wound and then tail sealed and cut to width to create a finished product roll of toilet tissue product. The resulting 2-ply toilet tissue product has a TS7 value of 6.7 dB V2 rms as measured by the Emtec Test Method, and a pilling of 8,700 mm3 as measured by the Pilling Test Method.

The randomly bonded, Inventive Sample 3 also creates a less textured, smoother surface as measured using optical profilometry. FIG. 13 compares the optical profilometry results of a base wet laid substrate, a polysaccharide layer thermal bonded to a wet laid substrate (Comparative Sample 1), and a polysaccharide layer randomly bonded to a wet laid substrate (Inventive Sample 3). The base wet laid substrate with no polysaccharide was prepared using a papermaking process as described in the Non-Limiting Examples of Making a First Web Material. The wet laid substrate with no polysaccharide has the highest Sa values which means the roughest surface (47.7 microns), followed by the thermal bonding polysaccharide on wet laid (43.0 microns), and the random bonding polysaccharide on wet laid providing the smoothest surface with the lowest Sa (30.5 microns).

The reason Inventive Sample 3 created a tissue product with low pilling without requiring a discrete bonding process was the polysaccharide filaments begin to exhibit tack and adhesion when they are not fully dried and laid down in a high humidity environment. The Dahlquist criterion states that a material will act as a pressure sensitive adhesive when it's storage modulus (G′) drops below a critical value. Because water acts as a plasticizer for the polysaccharide, the material's G′ will decrease with not only temperature, as observed in thermoplastic polymers, but also with water content. FIG. 14 shows how G′ varies as measured by the Modulus vs Relative Humidity and Temperature Test Method for the PVOH filaments with both relative humidity (RH) and temperature.

As shown in FIG. 14, Inventive Samples' G′ decreases significantly at higher RH, and furthermore as temperature increases, G′ drops at and even lower RH. As the drying air temperature and drying air flow are reduced during spinning, the RH of the forming environment increases which results in a lower G′, and thus the fibers will have more tack and stick to the wet laid cellulosic paper.

When the polysaccharide filaments are formed under different RH conditions, a ply bond method can be used to measure how strongly the layer of polysaccharide is bound to the wet laid substrate. When the fibers are fully dried, and the RH is relatively low when the fibers are formed, the ply bond is also low (9.7 g) because there is very little adhesion between the two layers as described in Comparative Sample 1. Consequently, a discrete bonding process, such as thermal bonding, would be required to sufficiently attach the polysaccharide layer to the cellulosic structure. Conversely, when the drying temperature and/or flow are reduced in the inventive example, the RH is relatively higher, and the ply bond is also higher (17.0 g) as measured by the Ply bond Test Method due to increased adhesion between the layers.

Sample 4—Comparative Sample—Non Thermal Bonded and Random Bonded with Low Drying and High Forming with Addition of a Fast-Wetting Surfactant to the Melt. Demonstrate how Fast Wetting Surfactants can Over Dry the Fibers and Prevent Tacky Laydown.

In a 40:1 APV Baker twin-screw extrude (Baker Perkins Co., Grand Rapids, MI) with eight temperature zones, 162 g/min of Purity Gum Ultra Food Starch Modified Corn Starch from Ingredion was mixed with 53 g/min water in Zone 1, using the temperature profile shown in TABLE 2. This mixture was then conveyed down the barrel through zones 2 through 8 at a screw speed of 500 RPM, where a second water injection of 97 g/min was introduced at zone 6. After exiting the extruder, the material was a homogeneous, uniform melt-processed polysaccharide composition with a water content of 40%. The water content was determined by collecting a melt sample in a plastic syringe and then ejecting the melt sample from the syringe onto an aluminum weight dish. The dish was weighed before and after drying in an oven overnight at 110 °C to determine how much water was in the original sample. The extruder barrel temperature setpoints for each zone are shown below in TABLE 2. After the extruder, a fast-wetting surfactant was added in-line using a static mixer at a composition of 1.0 wt % relative to the polysaccharide solids.

The temperature of the melt exiting the 40:1 extruder was between 121 and 132 °C. The melt temperature was measured with an in-line thermocouple. From the extruder, the melt was fed to a Zenith gear pump, Model #60-20000-2366-4 (Zenith Precision Metering, Monroe, NC), and the pump metered the melt to two static mixers where an additional 179 g/min of water was added. The melt composition at this point in the process was 58% water and 42% polysaccharide. From the static mixers, the polysaccharide melt composition was pumped to a melt blowing spinneret via a melt pump (Zenith gear pump, Model 5 #60-20000-2366-4).

A plurality of polysaccharide filaments was attenuated with a steam saturated air stream at 74 °C and 88% relative humidity to form a layer of filaments between 1 and 2 gsm that was collected either directly onto a forming belt or onto a differential density wet laid cellulose structure with a micro pattern of knuckles and pillows. The fibers were formed in a relatively high RH environment with a high forming as the Inventive Sample 3. However, since the fiber composition included 1.0 wt % of a fast-wetting surfactant, the water content of the spun filament layer was 0.7 wt % using the Filament Moisture Content Test Method, like Comparative Sample 2. The ply bond strength between the layer of PVOH filaments and the wet laid cellulosic structure was relatively low because there is very little adhesion between the polysaccharide filaments and the wet laid substrate. The layered substrate was not bonded with a high temperature, high pressure patterned nipped roll and wound to produce a parent roll.

This parent roll was unwound and combined and embossed with a wet-laid fibrous structure ply from a wet laid fibrous structure parent roll using glue to form a 2-ply embossed layered fibrous structure, such as a 2-ply toilet tissue product. A surface softener was then added from 5 to 20 lb/tne to the embossed side of the tissue product using a slot coater. The 2-ply toilet tissue product was wound and then tail sealed and cut to width to create a finished product roll of toilet tissue product. The resulting 2-ply toilet tissue product had a TS7 value of 6.5 dB V2 rms as measured by the Emtec Test Method and a Total Pilling Volume value of >10,000 mm3 as measured by the Pilling Test Method.

Sample 5—Comparative Sample—Thermal Bonded and Random Bonded with Low Drying and High Forming. Demonstrate how the Over-Bonded Structure does not have Desirable Surface Feel

A polysaccharide melt composition was prepared and pumped to a melt blowing die similarly to Sample 1, and the polysaccharide filaments were attenuated in a high RH environment similarly to Inventive Sample 3 such that the filaments have a low G′ and have good adhesion to the wet laid cellulosic structure. Unlike Inventive Sample 3, after formation, the layered structure was thermal bonded with a high temperature, high pressure patterned nipped roll at 300 °F and 325 psi to sufficiently attach the layers together. The thermal bonded substrate was wound about a core to produce a parent roll. This resulting substrate was both randomly bonded and discretely bonded.

This parent roll was unwound and combined and embossed with a wet-laid fibrous structure ply from a wet laid fibrous structure parent roll using glue to form a 2-ply embossed layered fibrous structure, such as a 2-ply toilet tissue product. A surface softener was then added from 5 to 20 lb/tne to the embossed side of the tissue product using a slot coater. The 2-ply toilet tissue product was wound and then tail sealed and cut to width to create a finished product roll of toilet tissue product. The resulting 2-ply toilet tissue product had an undesirable TS7 value of 9.6 dB V2 rms as measured by the Emtec Test Method, and a pilling value of less than 9,900 mm3 as measured by the Pilling Test Method. The relatively high TS7 value is because the substrate is over bonded with random and discrete bond sites.

Sample 6-Inventive sample-Non thermal bonded and random bonded with low drying and high forming with addition of 0.5 wt % of a fast-wetting surfactant to the melt. Demonstrate how filaments made with low levels of fast-wetting surfactants demonstrate tacky laydown and have the desired combination of surface and feel and pilling.

A polysaccharide melt composition was prepared and pumped to a melt blowing die similarly to Sample 4 except a fast-wetting surfactant was added in line to the polysaccharide melt after the extruder at a concentration of 0.5 wt % relative to the polysaccharide solids. A plurality of polysaccharide filaments was attenuated with a steam saturated air stream at 74 °C and 88% relative humidity to form a layer of filaments between 1 and 2 gsm that is collected either directly onto a forming belt or onto a differential density wet laid cellulose structure with a micro pattern of knuckles and pillows. The fibers were formed in a relatively high RH environment by drying them using air at 100 °C temperature and 570 m3/hr flowrate. Furthermore, a high forming air flow rate of 1020 m3/hr was employed to create a negative pressure differential at the consumer facing outer surface of the substrate. The water content of the spun filament layer was 3.1 wt % using the Filament Moisture Content Test Method. The ply bond strength between the layer of the polysaccharide filaments and the wet laid cellulosic structure was relatively high because there is good adhesion between the blended polysaccharide fibers and the wet laid substrate. The layered substrate is not bonded with a high temperature, high pressure patterned nipped roll and wound to produce a parent roll.

This parent roll was unwound and combined and embossed with a wet-laid fibrous structure ply from a wet laid fibrous structure parent roll using glue to form a 2-ply embossed layered fibrous structure, such as a 2-ply toilet tissue product. A surface softener was then added from 5 to 20 lb/tne to the embossed side of the tissue product using a slot coater. The 2-ply toilet tissue product was wound and then tail sealed and cut to width to create a finished product roll of toilet tissue product. The resulting 2-ply toilet tissue product has a TS7 value of 6.7 dB V2 rms as measured by the Emtec Test Method, and a pilling of 8,700 mm3 as measured by the Pilling Test Method.

The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as “40 mm” is intended to mean “about 40 mm.”

Every document cited herein, including any cross referenced or related patent or application and any patent application or patent to which this application claims priority or benefit thereof, is hereby incorporated herein by reference in its entirety unless expressly excluded or otherwise limited. The citation of any document is not an admission that it is prior art with respect to any invention disclosed or claimed herein or that it alone, or in any combination with any other reference or references, teaches, suggests or discloses any such invention. Further, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall govern.

While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended to cover in the appended claims all such changes and modifications that are within the scope of this invention.

Claims

1. A fibrous structure comprising a first web material and a consumer facing outer surface comprising a surface material different from the first web material, wherein the surface material comprises a polysaccharide fiber composition bonded to the first web material; wherein the fibrous structure has a pilling less than 10,000 mm3.

2. The fibrous structure according to claim 1 having an Sa of from about 25 μm to about 45 μm, as determined using the Surface Topography Test Method described herein.

3. The fibrous structure according to claim 1 having an Sq of from about 30 μm to about 60 μm, as determined using the Surface Topography Test Method described herein.

4. The fibrous structure according to claim 1, wherein the polysaccharide fiber composition is randomly bonded to the outer surface of the first web material.

5. The fibrous structure according to claim 1, wherein the TS7 value is from about 3 dB V2 rms to about 10 dB V2 rms.

6. The fibrous structure according to claim 1, wherein the TS7 value is from about 3 dB V2 rms to about 8 dB V2 rms.

7. The fibrous structure according to claim 1, wherein the TS7 value is from about 3.5 dB V2 rms to about 7 dB V2 rms.

8. The fibrous structure according to claim 1, wherein the pilling is from about 1 mm3 to about −1300 mm3.

9. The fibrous structure according to claim 1, wherein the pilling is from about 1 mm3 to about 1100 mm3.

10. The fibrous structure according to claim 1, wherein the pilling is from about 1 mm3 to about 900 mm3.

11. The fibrous structure according to claim 1, wherein the pilling is from about 1 mm3 to about 750 mm3.

12. The fibrous structure according to claim 1, wherein the pilling is from about 100 mm3 to about 700 mm3.

13. The fibrous structure according to claim 1, wherein the pilling is from about 100 mm3 to about 600 mm3.

14. The fibrous structure according to claim 1, wherein the polysaccharide composition comprises a plasticizer.

15. The fibrous structure according to claim 1, wherein the polysaccharide fiber composition is a filament.

16. The fibrous structure according to claim 1 wherein the first web material comprises a plurality of fibrous elements.

17. The fibrous structure according to claim 16 wherein at least one of the fibrous elements comprises a fiber.

18. The fibrous structure according to claim 17 wherein the fiber comprises a pulp fiber.

19. The fibrous structure according to claim 17 wherein the fiber comprises a non-naturally occurring fiber.

20. The fibrous structure according to claim 19 wherein the non-naturally occurring fiber comprises a polysaccharide.

21. The fibrous structure according to claim 20 wherein the polysaccharide is selected from the group consisting of: cellulose, cellulose derivatives, starch, starch derivatives, hemicelluloses, hemicelluloses derivatives, and mixtures thereof.

22. The fibrous structure according to claim 16 wherein at least one of the fibrous elements comprises a filament.

23. The fibrous structure according to claim 1 wherein the first web material comprises a wet laid fibrous structure ply.

24. The fibrous structure according to claim 1 wherein the ply bond of the polysaccharide fiber composition to the first web material is greater than 2.0 g.

25. The fibrous structure according to claim 1 wherein the ply bond of the polysaccharide fiber composition to the first web material is from about 1.0 g to about 15.0 g.

26. The fibrous structure according to claim 1 wherein the ply bond of the polysaccharide fiber composition to the first web material is from about 5.0 g to about 10.0 g.

27. A fibrous structure comprising a first web material and a surface comprising a surface material different from the first web material, wherein the surface material comprises a polysaccharide fiber composition;

wherein the polysaccharide fiber composition at a temperature of from about 65 °C to about 90 °C and relative humidity of from about 20% RH to about 50% RH has a modulus of less than 20 GPa.

28. The fibrous structure according to claim 26 wherein the polysaccharide fiber composition has a water content of from about 1% to about 25%.

29. The fibrous structure according to claim 26, wherein the polysaccharide fiber composition is a filament.

30. The fibrous structure according to claim 26 wherein the first web material comprises a plurality of fibrous elements.

31. The fibrous structure according to claim 29 wherein at least one of the fibrous elements comprises a fiber.

32. The fibrous structure according to claim 30 wherein the fiber comprises a pulp fiber.

33. The fibrous structure according to claim 30 wherein the fiber comprises a non-naturally occurring fiber.

34. The fibrous structure according to claim 32 wherein the non-naturally occurring fiber comprises a polysaccharide.

35. The fibrous structure according to claim 33 wherein the polysaccharide is selected from the group consisting of: cellulose, cellulose derivatives, starch, starch derivatives, hemicelluloses, hemicelluloses derivatives, and mixtures thereof.

36. The fibrous structure according to claim 29 wherein at least one of the fibrous elements comprises a filament.

37. The fibrous structure according to claim 26 wherein the first web material comprises a wet laid fibrous structure ply.

38. The fibrous structure according to claim 29 wherein at least one of the fibrous elements comprises a filament.

Patent History
Publication number: 20260348065
Type: Application
Filed: Apr 9, 2026
Publication Date: Nov 5, 2026
Inventors: Matthew Gary MCKEE (Cincinnati, OH), Mark Charles RUEVE (North Bend, OH), Patricia Callanan THOMAS (Wyoming, OH), Kevin James WALSH (Cincinnati, OH), William Ryan FALTA (Batavia, OH), Joerg KLEINWAECHTER (Loveland, OH), Frederick Scott BRITTON (Cincinnati, OH), Stephen Michael BEAUDION (Cincinnati, OH), Michael Joseph RODDY (Cincinnati, OH)
Application Number: 19/642,974
Classifications
International Classification: D04H 3/16 (20060101); D04H 1/26 (20120101); D04H 1/425 (20120101); D04H 1/4309 (20120101); D04H 1/4382 (20120101); D04H 1/559 (20120101); D21H 19/10 (20060101); D21H 27/00 (20060101);